Dual-phase composite ferrite material for X-band self-biasing device and preparation method thereof
By combining the hard magnetic phase with the soft magnetic phase and the introduction of dopants, the magnetization resistance and dielectric properties of the two-phase composite ferrite material are controlled, which solves the problem that the X-band self-biased device materials in the existing technology are difficult to achieve both. The problems of anisotropic field, high coercive force and residual magnetization ratio have achieved appropriate magnetoelectric properties and small, lightweight and integrated development.
Patent Information
- Application Number
- CN202211287484.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-20
AI Technical Summary
It is difficult for existing ferrite materials for X-band self-biased devices to have suitable anisotropic field, high coercive force and residual magnetization ratio characteristics, which limits the self-biasing characteristics and the development of small, lightweight and integrated microwave devices. .
Dual-phase composite ferrite materials are used to "graft" the high Mr/Ms and Hc characteristics of the hard magnetic phase onto the high-dielectric and low-loss soft magnetic phase. Through the exchange coupling effect of the hard magnetic phase and the soft magnetic phase and the incoherent phase The boundary structure, combined with the introduction of dopants, regulates the magnetization resistance and dielectric properties of the material to achieve appropriate anisotropic fields, coercive forces and dielectric constants.
It achieves suitable saturation magnetization, anisotropic field, coercive force, remanence ratio and dielectric constant characteristics of the dual-phase composite ferrite material, supports high internal field maintenance and low-frequency applications of X-band self-biased devices, and reduces It reduces the insertion loss and volume of the device and promotes the development of small, lightweight and integrated systems.
Smart Images

Figure CN115579203B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferrite material preparation, and particularly relates to a dual-phase composite ferrite material for an X-band self-biasing device and a preparation method thereof. Background Art
[0002] With the continuous improvement of monolithic microwave integrated circuit (MMIC) technology, microwave devices such as circulators and isolators are also developing towards small, lightweight and integrated directions. Microwave devices designed based on the gyromagnetic properties of ferrite play a vital role in information sharing and inter-stage isolation, and become the key to determining the reliability and stability of electronic communication systems. According to the crystal structure, ferrite gyromagnetic materials for microwave devices can be divided into three types: spinel, garnet and magnetoplumbite. Due to the difference in material properties, the applied frequencies are also different; for example, garnet ferrite has both suitable saturation magnetization intensity and low loss characteristics, and is widely used in X-band microwave device design. However, in order to realize the function of microwave devices, external magnetic steel is usually required to provide a bias magnetic field, which greatly increases the weight and volume of microwave devices, which is not conducive to the small, lightweight and integrated development of the entire system.
[0003] Among the three ferrite gyromagnetic materials, M-type hexagonal ferrite (SrM) has the characteristics of high coercive force, high anisotropy field and high remanence ratio. High coercive force can maintain the permanent magnetic properties of hexagonal ferrite; high remanence ratio can make the magnetic moment tend to precess in the direction of strong anisotropy, so that the magnetic moment can produce ferromagnetic resonance with microwave / millimeter wave in the absence of an external steady magnetic field or a very small steady magnetic field. The above-mentioned unique advantages of M-type hexagonal ferrite materials can provide a self-bias field for the operation of microwave devices, completely get rid of the constraints of external magnetic steel, and realize self-bias characteristics. However, due to the high anisotropy field, the application frequency of M-type hexagonal ferrite materials is generally higher than the Ka band, and it cannot be applied to the design of X-band microwave devices. Therefore, the present invention combines the respective advantages of garnet ferrite and M-type hexagonal ferrite to develop a two-phase composite ferrite material for X-band self-bias devices, which is of great significance to the realization of the self-bias characteristics of X-band microwave devices.
[0004] In response to the current research on microwave ferrite materials for X-band self-biased devices, the University of Jordan (Mater. Res. Bull., 2016, 74: 192-210) published a BaFe 11.6 Cu 0.4 O 19 Ferrite material performance indicators: specific saturation magnetization intensity σ s =68.5g / emu, remanence ratio M r / M s =0.32, coercive force H c =459Oe, anisotropy field H a= 10.7 kOe, the ferromagnetic resonance line width ΔH is not published, although the H of hexagonal ferrite material a Greatly reduced, but the material M r / M s and H c The low value is not conducive to maintaining the self-bias characteristic. A BaSc 0.1 Fe 11.9 O 19 The performance index of ferrite materials is: saturation magnetization intensity 4πM s =4700Gs, remanence ratio M r / M s =0.65, coercive force H c =2400Oe, anisotropy field H a =7.8kOe, the ferromagnetic resonance line width ΔH is not published, although the material has a suitable H c With H a , but M r / M s The performance index of a La, Sc-substituted M-type hexagonal ferrite material published in patent CN11204731A is: saturation magnetization intensity 4πM s >3790Gs, remanence 4πM r >3415Gs, coercivity H c >550Oe, anisotropic field H a >13.6kOe, ferromagnetic resonance line width ΔH>389Oe, but the H c Lower, ΔH larger; Patent CN111732427B published a Ga-substituted hexagonal ferrite material performance index: saturation magnetization 4πM s >4167Gs, coercivity H c >2280Oe, remanence ratio M s / M r >0.88, anisotropy field H a >18.02kOe, ferromagnetic resonance line width ΔH>260Oe, although the material has a suitable M s / M r with ΔH, but H aIt is not difficult to see from the above results that although the anisotropy field of M-type hexagonal ferrite can be reduced by Sc, Cu plasma substitution, the magnetic properties are seriously deteriorated, which is not conducive to the design of X-band microwave devices. In addition, Nehru University of India (J. Alloys. Compd., 2018, 736: 266-275) published a sol-gel method to prepare BaM / YIG composite ferrite. As the YIG content increases, the anisotropy field H a The ferromagnetic resonance line width ΔH decreases from 2000Oe to 385Oe, but the coercive force H c <600Oe is relatively low, which is not conducive to maintaining the self-bias characteristics; Shaanxi University of Science and Technology (Mater. Res. Bull., 2014, 60: 195-200) published a sol-gel method for one-step synthesis of BaFe 12 O 19 / Y3Fe5O 12 Composite material performance index: coercivity H c =689Oe, specific saturation magnetization σ s =34.13emu / g, remanence ratio M r / M s =0.584, ferromagnetic resonance line width ΔH and anisotropy field H a Unpublished. Although the composite magnets synthesized by chemical methods can improve the microwave performance of the magnets to a certain extent, the preparation technology is complex, the reaction process is difficult to control, the pollution is large, and the magnet orientation is difficult, which makes them unsuitable for self-biased device applications.
[0005] Based on the above, it is difficult for existing ferrite materials for X-band self-bias devices to have suitable anisotropy field, high coercivity and remanence ratio characteristics. The present invention provides a dual-phase composite ferrite material for X-band self-bias devices and a preparation method thereof, which combines a hard magnetic phase with a high M r / M s and H c The properties are "grafted" onto the high-dielectric and low-loss soft magnetic phase to develop a two-phase composite ferrite material with suitable anisotropy field, high coercive force and remanence ratio, low ferromagnetic resonance linewidth and high dielectric constant. Summary of the invention
[0006] The purpose of the present invention is to solve the technical problem that the ferrite material for X-band self-bias device involved in the prior art is difficult to have suitable anisotropy field, high coercivity and remanence ratio characteristics, and to propose a dual-phase composite ferrite material for X-band self-bias device and a preparation method thereof. The developed material has suitable saturation magnetization intensity (4πM s ≥3028Gs), suitable anisotropic field (H a ≤11.56kOe), high coercivity (H c≥3754Oe), high remanence ratio (M r / M s ≥0.90), low ferromagnetic resonance linewidth (ΔH≤350Oe) and high dielectric constant (ε'≥23), making it suitable for X-band self-biased device design.
[0007] The core idea of the present invention is to convert the hard magnetic phase into high M r / M s and H c The characteristics are "grafted" onto the high-dielectric and low-loss soft magnetic phase. The main formula of the hard magnetic phase uses an appropriate amount of iron-deficient, high coercive force and remanence ratio CaLaCo to replace SrM ferrite; the main formula of the soft magnetic phase uses an appropriate amount of iron-deficient, high dielectric constant and low loss BiZrCaV to replace YIG ferrite. First of all, the hard magnetic phase has the characteristics of high remanence ratio and high coercive force. According to the anisotropy compensation mechanism, the soft magnetic phase with low anisotropy field is introduced to compensate the hard magnetic phase with high anisotropy field, which can effectively reduce the anisotropy field of the two-phase composite ferrite. And due to the exchange coupling between the soft magnetic phase and the hard magnetic phase, the two-phase composite ferrite still maintains a relatively high remanence ratio and coercive force. Secondly, during the preparation process, the soft magnetic phase is added to the hard magnetic phase pre-sintered material in the form of raw materials. On the one hand, during the secondary pre-sintering process of the mixture, the soft magnetic phase raw materials enriched around the hard magnetic phase particles will gradually react on the surface of the hard magnetic phase particles to generate soft magnetic phases, and "wrap" the hard magnetic phase. The contact area increases, which is conducive to the exchange coupling between the two phases. In addition, the soft magnetic phase generated on the surface of the hard magnetic phase particles will combine with the hanging bonds on the surface of the hard magnetic phase, making the combination of the two phases more stable and ensuring the uniformity of the distribution of the two phases. On the other hand, a non-coherent phase boundary is formed between the two phases. There is a transition zone with large composition fluctuations in this phase boundary, which will produce a large resistance to the displacement of the domain wall during the demagnetization process of the two-phase composite ferrite. Together with the exchange coupling, the two-phase composite ferrite maintains a high coercive force. Thirdly, Bi 3+ 、V 5+ The fluxing effect can reduce the sintering temperature of YIG ferrite to match the sintering temperature of SrM ferrite, and can also make the dual-phase composite ferrite densified and sintered, reduce the porosity, which is beneficial to improve the remanence ratio and reduce the ferromagnetic resonance line width; during the sintering process, Bi 3+ The dielectric properties of the dual-phase composite ferrite can be improved by diffusing into the hexagonal ferrite lattice. 4+ 、V 5+ The diffusion of high-valent ions such as Fe 2+The generation of dual-phase composite ferrites can improve the resistivity and reduce microwave dielectric loss. Finally, dopants such as CaCO3, Bi2O3, SiO2, H3BO3 and nano-BaTiO3 ceramic powder are introduced. Dopants such as CaCO3, Bi2O3, SiO2 and H3BO3 regulate the grain and grain boundary characteristics of dual-phase composite ferrites through the crystal promotion / crystallization inhibition mechanism, narrow the particle size distribution, improve the orientation degree, and improve the microscopic properties and magnetic properties of the sintered body. Nano-BaTiO3 ceramic powder can increase grain boundary resistance, improve resistivity, and reduce microwave dielectric loss. That is: through the control of the anisotropy compensation mechanism, low anisotropy YIG ferrite is introduced to reduce the anisotropy field of the dual-phase composite ferrite material; through two pre-sintering, the high remanence ratio and coercive force of the dual-phase composite ferrite are achieved based on exchange coupling and incoherent phase boundary magnetization resistance; through the main formula of YIG ferrite, Bi 3+ 、V 5+ The low-temperature fluxing effect of Zr increases the densification degree of the dual-phase composite ferrite and reduces the ferromagnetic resonance line width. 4+ 、V 5+ The diffusion of nano BaTiO3 ceramic powder and the introduction of dopants improve the grain / grain boundary resistance characteristics of the dual-phase composite ferrite. 3+ The diffusion of CaCO3, Bi2O3, SiO2, and H3BO3 dopants improves the dielectric properties of the dual-phase composite ferrite; through the crystal inhibition / crystallization promotion mechanism of CaCO3, Bi2O3, SiO2, and H3BO3 dopants, the grain boundary characteristics are regulated, the orientation degree is increased, and the microstructure and magnetic properties of the dual-phase composite ferrite are improved.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0009] A dual-phase composite ferrite material for an X-band self-biasing device, the dual-phase composite ferrite material comprising SrM ferrite, YIG ferrite and a dopant; the components of the SrM ferrite are: 3.82-10.34 mol% SrCO3, 0.74-4.85 mol% CaCO3, 2.33-8.17 mol% La2O3, 1.45-6.49 mol% Co2O3, 76.67-85.14 mol% Fe2O 3. The components of the YIG ferrite are: 17.43-30.22 mol% Y2O3, 5.22-10.41 mol% Bi2O3, 5.56-10.68 mol% ZrO2, 5.23-11.32 mol% CaCO3, 3.2-14.2 mol% V2O5, 39.57-46.96 mol% Fe2O3, and the weight ratio of YIG ferrite to SrM ferrite is 1:(0.11-9);
[0010] The weight percentage of the dopant in the composite ferrite material is: 0.2-0.6wt.% SiO2, 0.1-0.8wt.% H3BO3, 0.3-1.5wt.% CaCO3, 0.4-1.2wt.% Bi2O3, 0.4-1.4wt.% BaTiO3.
[0011] A method for preparing a dual-phase composite ferrite material for an X-band self-biasing device comprises the following steps:
[0012] Step 1: Ingredients
[0013] Using SrCO3, CaCO3, La2O3, Co2O3 and Fe2O3 as raw materials, the materials are weighed and mixed according to the ratio of "3.82-10.34 mol% SrCO3, 0.74-4.85 mol% CaCO3, 2.33-8.17 mol% La2O3, 1.45-6.49 mol% Co2O3, 76.67-85.14 mol% Fe2O3" to obtain initial SrM ferrite powder;
[0014] Step 2: First ball milling
[0015] The initial powder obtained in step 1 is mixed evenly in a ball mill for 8 to 20 hours;
[0016] Step 3: Pre-burning
[0017] The primary ball mill material obtained in step 2 is dried, sieved, and pre-fired at 1100-1400° C., with a heating rate of 0.5-1.6° C. / min and a holding time of 1.5-6 h to obtain a SrM ferrite pre-fired material;
[0018] Step 4: Secondary ball milling
[0019] Y2O3, Bi2O3, ZrO2, CaCO3, V2O5 and Fe2O3 are used as raw materials, and the ingredients are prepared in the proportion of "17.43-30.22mol% Y2O3, 5.22-10.41mol% Bi2O3, 5.56-10.68mol% ZrO2, 5.23-11.32mol% CaCO3, 3.2-14.2mol% V2O5 and 39.57-46.96mol% Fe2O3" to obtain YIG ferrite; according to the weight ratio of YIG ferrite to SrM ferrite initial powder being 1:(0.11-9), YIG ferrite is added to SrM ferrite pre-sintered material, and ball milling is performed to mix evenly, and the ball milling time is 5-21h;
[0020] Step 5: Secondary pre-burning
[0021] The secondary ball mill obtained in step 4 is dried and pre-fired at 1000-1300° C. for 1-7 hours;
[0022] Step 6: Doping
[0023] Adding dopants to the secondary pre-sintered material obtained in step 5, wherein the weight percentage of the dopants in the composite ferrite material is: 0.2-0.6wt.% SiO2, 0.1-0.8wt.% H3BO3, 0.3-1.5wt.% CaCO3, 0.4-1.2wt.% Bi2O3, and 0.4-1.4wt.% BaTiO3;
[0024] Step 7: Three-time ball milling
[0025] The mixed powder obtained in step 6 is ball-milled in a ball mill for 15 to 28 hours to be uniformly mixed, and the particle size of the powder is controlled between 0.6 and 1.0 μm;
[0026] Step 8: Molding
[0027] Dehydrate the tertiary ball mill obtained in step 7, control the water content of the slurry to be between 18wt% and 35wt% after dehydration, and then press-form the slurry in a magnetic field forming machine, wherein the forming magnetic field is 1.3 to 1.6T and the forming pressure is 85 to 130MPa;
[0028] Step 9: Sintering
[0029] The blank obtained by pressing in step 8 is sintered at a sintering temperature of 1050-1200° C. for a holding time of 3-8 hours. After sintering, a dual-phase composite ferrite material for an X-band self-biasing device can be obtained.
[0030] The performance test of the two-phase composite ferrite material obtained in step 9 is carried out: saturation magnetization intensity 4πM s , residual magnetization 4πM r , Remanence ratio M r / M s , coercive force H c The test was conducted using the American LakeShore 8604 vibrating sample magnetometer, the dielectric constant ε' was tested using the American Keysight E4991B impedance analyzer, the ferromagnetic resonance line width ΔH was tested using the American Agilent N5227A vector network analyzer, and the anisotropic field H a It is derived from Kittel's formula.
[0031] The final technical indicators of the dual-phase composite ferrite material prepared by the present invention are as follows:
[0032] Saturation magnetization 4πM s ≥3028Gs;
[0033] Remanence ratio M r / M s ≥0.90;
[0034] Coercivity H c ≥3754Oe;
[0035] Anisotropy field H a ≤11.56kOe;
[0036] Line width ΔH ≤ 350Oe;
[0037] Dielectric constant ε'≥23.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The invention provides a dual-phase composite ferrite material for an X-band self-bias device, which has a suitable saturation magnetization intensity (4πM s ≥3028Gs), suitable anisotropic field (H a ≤11.56kOe), high coercivity (H c ≥3754Oe), high remanence ratio (M r / M s ≥0.90), low ferromagnetic resonance linewidth (ΔH≤350Oe) and high dielectric constant (ε'≥23). High coercivity to remanence ratio can maintain high internal field, which is conducive to the realization of self-bias characteristics; suitable anisotropy field can make the self-bias device work in the X-band, which is conducive to the low-frequency application of self-bias devices; low ferromagnetic resonance linewidth is conducive to reducing the insertion loss of self-bias devices; high dielectric constant can further reduce the weight and volume of self-bias devices, which is conducive to the development of small, lightweight and integrated whole system. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is the hysteresis loop of the dual-phase composite ferrite material obtained in Example 1;
[0041] Figure 2 This is a ferromagnetic resonance line width fitting diagram of the dual-phase composite ferrite material obtained in Example 1;
[0042] Figure 3 This is a scanning electron microscope photograph of the dual-phase composite ferrite material obtained in Example 1;
[0043] Figure 4 This is a scanning electron microscope photograph of the dual-phase composite ferrite material obtained in Example 2;
[0044] Figure 5 This is a scanning electron microscope photograph of the dual-phase composite ferrite material obtained in Example 3;
[0045] Figure 6 This is a scanning electron microscope photograph of the dual-phase composite ferrite material obtained in Example 4. DETAILED DESCRIPTION
[0046] Aiming at the application requirements of small, lightweight and integrated X-band microwave devices, the present invention provides a dual-phase composite ferrite material for X-band self-bias devices and a preparation method thereof, which overcomes the technical difficulty that the existing ferrite materials for X-band self-bias devices are difficult to have suitable anisotropic field, high coercive force and remanence ratio characteristics. r / M s and H c The characteristics are "grafted" onto high-dielectric and low-loss YIG ferrite. Two pre-sinterings are used on the basis of the solid phase method to ensure that the reaction is controllable and the uniformity of the two-phase distribution is achieved. The anisotropy compensation mechanism, exchange coupling theory, magnetization resistance mechanism, material surface interface theory, and diffusion theory are used to deeply analyze the mechanism of the influence of the introduction of YIG on the performance of the two-phase composite ferrite. Combining the sintering kinetics and the crystal promoting / crystallization inhibiting mechanism, the influence of additives on the microstructure and magnetic properties of the two-phase composite ferrite is clarified, the best main formula and additive formula are formulated, and the process is optimized. Finally, a two-phase composite ferrite material with suitable anisotropy field, high coercivity and remanence ratio, low ferromagnetic resonance linewidth, and high dielectric constant characteristics is developed.
[0047] Embodiments 1 to 4
[0048] Step 1: Ingredients
[0049] SrM ferrite uses SrCO3, CaCO3, La2O3, Co2O3, and Fe2O3 as raw materials, and the initial SrM ferrite powder is prepared according to the proportions shown in the following table. The SrM ferrite formula in Examples 1 to 4 is shown in the following table:
[0050]
[0051] Step 2: First ball milling
[0052] The initial powder obtained in step 1 was mixed evenly in a planetary ball mill for 12 h;
[0053] Step 3: Pre-burning
[0054] The primary ball milled material obtained in step 2 is dried, sieved, and pre-fired at 1250° C. with a heating rate of 0.8° C. / min and a holding time of 4 h to obtain a SrM ferrite pre-fired material;
[0055] Step 4: Secondary ball milling
[0056] YIG ferrite uses Y2O3, Bi2O3, ZrO2, CaCO3, V2O5, and Fe2O3 as raw materials, and the ingredients are prepared according to the proportions shown in the following table. The YIG ferrite formulas in Examples 1 to 4 are shown in the following table:
[0057]
[0058] According to the weight ratio of the initial powder of YIG ferrite to SrM ferrite of 1:0.82, YIG ferrite was added to the pre-sintered SrM ferrite, and the mixture was evenly milled in a planetary ball mill for 16 hours.
[0059] Step 5: Secondary pre-burning
[0060] The secondary ball milled material obtained in step 4 is dried and pre-fired at 1100° C. for 3 h;
[0061] Step 6: Doping
[0062] Add dopants to the secondary pre-sintered material obtained in step 5, and the weight percentage of the dopants in the composite ferrite material is: 0.4wt.% SiO2, 0.6wt.% H3BO3, 1.2wt.% CaCO3, 0.8wt.% Bi2O3, and 0.7wt.% BaTiO3;
[0063] Step 7: Three-time ball milling
[0064] The mixed powder obtained in step 6 is ball-milled in a planetary ball mill for 18 hours to be uniformly mixed, and the particle size of the powder is controlled between 0.6 and 1.0 μm;
[0065] Step 8: Molding
[0066] Dehydrate the tertiary ball mill obtained in step 7, control the water content of the slurry to be between 30wt% and 35wt% after dehydration, and then press-form the slurry in a magnetic field forming machine, wherein the forming magnetic field is 1.4T and the forming pressure is 120MPa;
[0067] Step 9: Sintering
[0068] The blank obtained by pressing in step 8 is sintered at a sintering temperature of 1160° C. and a holding time of 5 hours. After sintering, a dual-phase composite ferrite material for an X-band self-bias device can be obtained.
[0069] The performance test of the two-phase composite ferrite material obtained in step 9 is carried out: saturation magnetization intensity 4πM s , residual magnetization 4πM r , Remanence ratio M r / M s , coercive force H cThe test was conducted using the American LakeShore 8604 vibrating sample magnetometer, the dielectric constant ε' was tested using the American Keysight E4991B impedance analyzer, the ferromagnetic resonance line width ΔH was tested using the American Agilent N5227A vector network analyzer, and the anisotropic field H a It is derived from Kittel's formula.
[0070] Based on the above-mentioned process, the performance parameters of the dual-phase composite ferrite material of Examples 1 to 4 are as follows:
[0071]
Claims
1. A dual-phase composite ferrite material for an X-band self-biasing device, It is characterized in that The dual-phase composite ferrite material comprises SrM ferrite, YIG ferrite and dopant; the composition of the SrM ferrite is: 3.82-10.34 mol% SrCO 3 , 0.74~4.85mol%CaCO 3 、2.33~8.17mol%La 2 O 3 、1.45~6.49mol%Co 2 O 3 、76.67~85.14mol%Fe 2 O 3 The composition of the YIG ferrite is: 17.43-30.22 mol% Y 2 O 3 、5.22~10.41mol%Bi 2 O 3 5.56~10.68mol%ZrO 2 5.23~11.32mol%CaCO 3 、3.2~14.2mol%V 2 O 5 、39.57~46.96mol%Fe 2 O 3 , the weight ratio of YIG ferrite to SrM ferrite is 1:(0.11~9); The weight percentage of the dopant in the composite ferrite material is: 0.2-0.6wt.% SiO 2 、0.1~0.8wt.%H 3 BO 3 、0.3~1.5wt.%CaCO 3 、0.4~1.2wt.%Bi 2 O 3 、0.4~1.4wt.%BaTiO 3 .
2. A method for preparing a dual-phase composite ferrite material for an X-band self-biasing device, It is characterized in that The following steps are involved: Step 1: Ingredients SrCO 3 、CaCO 3 ,La 2 O 3 、Co 2 O 3 , Fe 2 O 3 As raw materials, according to "3.82~10.34mol%SrCO 3 , 0.74~4.85mol%CaCO 3 、2.33~8.17mol%La 2 O 3 、1.45~6.49mol%Co 2 O 3 、76.67~85.14mol%Fe 2 O 3 " and weighing and mixing the materials to obtain initial SrM ferrite powder; Step 2: First ball milling The initial powder obtained in step 1 is mixed evenly in a ball mill for 8 to 20 hours; Step 3: Pre-burning The primary ball mill material obtained in step 2 is dried, sieved, and pre-fired at 1100-1400° C., with a heating rate of 0.5-1.6° C. / min and a holding time of 1.5-6 h to obtain a SrM ferrite pre-fired material; Step 4: Secondary ball milling Y 2 O 3 、Bi 2 O 3 、ZrO 2 、CaCO 3 、V 2 O 5 , Fe 2 O 3 As raw materials, according to "17.43~30.22mol%Y 2 O 3 、5.22~10.41mol%Bi 2 O 3 5.56~10.68mol%ZrO 2 5.23~11.32mol%CaCO 3 、3.2~14.2mol%V 2 O 5 、39.57~46.96mol%Fe 2 O 3 " to obtain YIG ferrite; according to the weight ratio of YIG ferrite to SrM ferrite initial powder being 1: (0.11-9), YIG ferrite is added to the SrM ferrite pre-sintered material, and ball milling is performed to mix evenly, and the ball milling time is 5-21h; Step 5: Secondary pre-burning The secondary ball mill obtained in step 4 is dried and pre-fired at 1000-1300° C. for 1-7 hours; Step 6: Doping Add a dopant to the secondary pre-sintered material obtained in step 5, and the weight percentage of the dopant in the composite ferrite material is: 0.2-0.6 wt.% SiO 2 、0.1~0.8wt.%H 3 BO 3 、0.3~1.5wt.%CaCO 3 、0.4~1.2wt.%Bi 2 O 3 、0.4~1.4wt.%BaTiO 3 ; Step 7: Three-time ball milling The mixed powder obtained in step 6 is ball-milled in a ball mill for 15 to 28 hours to be uniformly mixed, and the particle size of the powder is controlled between 0.6 and 1.0 μm; Step 8: Molding Dehydrate the tertiary ball mill obtained in step 7, control the water content of the slurry to be between 18wt% and 35wt% after dehydration, and then press-form the slurry in a magnetic field forming machine, wherein the forming magnetic field is 1.3 to 1.6T and the forming pressure is 85 to 130MPa; Step 9: Sintering The blank obtained by pressing in step 8 is sintered at a sintering temperature of 1050-1200° C. for a holding time of 3-8 hours. After sintering, a dual-phase composite ferrite material for an X-band self-biasing device can be obtained.