Preparation method and application of environmentally friendly inorganic powder dispersant
By controlling the ratio and process conditions of polyetherate and polycaprolactone polyol in the preparation of inorganic powder dispersants, combined with the use of specific fluoropolymer additives, the problems of uneven dispersion of inorganic powder and environmental protection are solved , improves the fluidity and compatibility of the dispersant, and meets the needs of environmental protection and performance improvement.
Patent Information
- Application Number
- CN202111589978.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-23
AI Technical Summary
Existing inorganic powder dispersants are unevenly dispersed in polymer materials and are prone to agglomeration, and many hyperdispersants contain toxic substances, which cannot completely solve environmental protection problems.
By mixing polyetherate and polycaprolactone polyol under nitrogen protection conditions, controlling the temperature and time of holding and cooling, and adding specific fluoropolymer additives, an environmentally friendly inorganic powder dispersant is prepared to avoid the generation of irritating odors. And improve the fluidity of masterbatch.
It achieves uniform dispersion of inorganic powder in the resin, improves dispersibility and compatibility, improves the mechanical properties and processing properties of the masterbatch, reduces the generation of irritating odors, and improves fluidity, satisfying environmental protection requirements. Require.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of dispersants, in particular to IPC classification number C08F222 / 06, and more particularly to a preparation method and application of an environmentally friendly inorganic powder dispersant. Background Art
[0002] In the field of polymer materials such as rubber, plastic, chemical fiber, and coatings, inorganic powders such as fillers or pigments are often added to give the materials excellent properties. However, due to the existence of an interface area between the resin matrix and the inorganic powder, the compatibility between the two is poor, which makes it impossible for the inorganic powder material to be evenly dispersed in the organic resin, and agglomeration is prone to occur.
[0003] For this reason, the emergence of hyperdispersants has a significant effect on the dispersion of inorganic powders. However, the dispersion ability of some hyperdispersants on the market is relatively weak, and some even contain a lot of toxic substances, which does not meet the current requirements for green environmental protection. Chinese patent CN201510102492 discloses an amphiphilic super dispersant and a preparation method thereof. Solution A is obtained by mixing oleic acid, maleic anhydride, methyl methacrylate, azobisisobutyronitrile and isopropanol. Solution A is added dropwise into an acetone solution in a N2 protected environment and under stirring. The acetone solution is heated in a water bath at 60 to 80°C. After the dropwise addition is completed, the solution is kept warm for 5 to 8 hours. The product is filtered, washed and dried to obtain a super dispersant. Nano copper powder and super dispersant are dissolved in an acetone solvent, ultrasonically dispersed, heated in a water bath at 60 to 80°C, stirred at high speed for 2 to 6 hours, filtered, washed and dried to obtain an amphiphilic super dispersant. The dispersant has super strong dispersing ability. By using isopropanol as a chain transfer agent, the non-environmental protection of using mercaptan as a chain transfer agent is avoided. However, azobisisobutyronitrile is still used in the dispersant, which may produce toxic gases during the processing and does not completely solve the environmental protection problem. Summary of the invention
[0004] In view of the above-mentioned technical problems, the present invention provides a method for preparing an environmentally friendly inorganic powder dispersant, which comprises at least the following steps:
[0005] (1) mixing polyether ester and polycaprolactone polyol under nitrogen protection, and keeping the mixture warm for a certain period of time to obtain a mixture A;
[0006] (2) After cooling, a processing aid is added to the mixture A, and the dispersant is obtained after mixing.
[0007] In some embodiments, the insulation temperature in step (1) is 70-80°C.
[0008] Preferably, the insulation temperature in step (1) is 75°C.
[0009] In some embodiments, the insulation time in step (1) is 30-60 minutes.
[0010] Preferably, the insulation time in step (1) is 45 minutes.
[0011] In some embodiments, the cooling temperature in step (2) is 40-50°C.
[0012] Preferably, the cooling temperature in step (2) is 40-45°C.
[0013] More preferably, the cooling temperature in step (2) is 43°C.
[0014] In some embodiments, the mixing time in step (2) is 60-120 min.
[0015] Preferably, the mixing time in step (2) is 90 minutes.
[0016] In some embodiments, the weight ratio of the polyether ester to the polycaprolactone polyol is (0.6-1.5):1.
[0017] In some embodiments, the polycaprolactone polyol is a polycaprolactone triol having a number average molecular weight of 1000-3000.
[0018] Preferably, the number average molecular weight of the polycaprolactone triol is 2000.
[0019] More preferably, the polycaprolactone triol is purchased from Hubei Handafei Biotechnology Co., Ltd.
[0020] Preferably, the weight ratio of the polyether ester to the polycaprolactone polyol is 1.1:1.
[0021] In some embodiments, the preparation of the polyether ester comprises: mixing polyether polyol and acid anhydride, heating and keeping the temperature for a period of time, discharging, cooling, and grinding to obtain the polyether ester.
[0022] In some embodiments, the molar ratio of the polyether polyol to the acid anhydride is 1:(1.05-1.2).
[0023] Preferably, the molar ratio of the polyether polyol to the acid anhydride is 1:1.15.
[0024] In some embodiments, the heating temperature is 100-120° C., and the insulation time is 2-4 hours.
[0025] Preferably, the heating temperature is 105° C. and the insulation time is 3 hours.
[0026] In some embodiments, the polyether polyol includes polyethylene glycol and / or polypropylene glycol.
[0027] Preferably, the polyether polyol comprises polyethylene glycol and polypropylene glycol in a weight ratio of (1-2):1.
[0028] More preferably, the polyether polyol comprises polyethylene glycol and polypropylene glycol in a weight ratio of 1.5:1.
[0029] In some embodiments, the polyethylene glycol has a number average molecular weight of 720-880 and a hydroxyl value of 127-156 mgKOH / g.
[0030] Preferably, the polyethylene glycol is purchased from Shanghai Lianji Chemical Co., Ltd., and the model is PEG800.
[0031] In some embodiments, the polypropylene glycol has a number average molecular weight of 3000 and a hydroxyl value of 34-42 mgKOH / g.
[0032] Preferably, the polypropylene glycol is purchased from Shanghai Lianji Chemical Co., Ltd., model number is PPG3000.
[0033] In some embodiments, the anhydride comprises maleic anhydride.
[0034] In some embodiments, the processing aid comprises a fluorine-containing polymer additive, and the fluorine content of the fluorine-containing polymer additive is 65-80%.
[0035] Preferably, the fluorine content of the fluorine-containing polymer auxiliary agent is 70-75%.
[0036] In some embodiments, the weight ratio of the fluorine-containing polymer auxiliary to the polycaprolactone polyol is 1:(1.4-1.8).
[0037] Preferably, the weight ratio of the fluorine-containing polymer additive to the polycaprolactone polyol is 1:1.6.
[0038] The present invention does not impose any special restrictions on the source of the fluorine-containing polymer additive, including but not limited to, the fluorine-containing polymer additive is purchased from Shangxi (Shanghai) Chemical Additive Co., Ltd., and the brand is Japan Daikin DA912.
[0039] During the preparation process of the inorganic powder dispersant, due to the influence of mechanical force or temperature, small molecular monomers may be generated, thereby causing unpleasant odors. After extensive research, the applicant found that by controlling the specific ratio of polyether ester and polycaprolactone polyol, as well as the temperature and time of heat preservation and cooling, especially controlling the weight ratio of polyether ester to polycaprolactone polyol to (0.6-1.5):1, and the heat preservation temperature in step (1) is 70-80°C, the heat preservation time is 30-60min, and the cooling temperature in step (2) is controlled to be 40-45°C and the mixing time is 60-120min, the generation of pungent odors during the preparation of the inorganic powder dispersant is well avoided, and it is more environmentally friendly. The applicant believes that the possible reason is that by controlling the multiple branches of the polyether ester and the polycaprolactone polyol to be tightly combined at multiple sites through physical bonding at a specific temperature and time, the breakage and decomposition between the segments are reduced, thereby avoiding the migration and precipitation of free small molecular monomers, so that the inorganic powder dispersant is more environmentally friendly throughout the preparation and use process. Although the applicant has avoided the generation of unpleasant odor by controlling the raw material ratio and process conditions, the applicant unexpectedly found that the fluidity of the masterbatch prepared by using the dispersant in the process of masterbatch preparation is low. At the same time, some masterbatches currently on the market also have the problem of poor fluidity, which prolongs the production cycle of the prepared plastic products and affects their appearance quality. For this reason, the applicant has made a lot of efforts and found that by adding a fluorine-containing polymer additive with a specific fluorine content to the dispersant and controlling the mixing time after adding, especially when the fluorine content is 70-75%, the fluidity of the prepared masterbatch can be improved. The applicant believes that the possible reason is that under this condition, the additive has a lower surface energy. When the dispersant is added to the masterbatch, on the one hand, the friction between the polymer molecules is reduced during the processing process, and the viscosity of the melt is reduced. On the other hand, the inorganic powder is more evenly dispersed, and the agglomerates are broken up under the action of shear force. The two aspects work together to give the prepared masterbatch better fluidity.
[0040] Another aspect of the present invention provides a method for preparing an environmentally friendly inorganic powder dispersant. The prepared dispersant is used for dispersing pigments and fillers in masterbatches.
[0041] Beneficial effects:
[0042] The present invention uses a specific preparation method to make the obtained inorganic powder dispersant have good fluidity, which can not only improve the dispersibility of the inorganic powder filled resin, but also well improve the compatibility between the inorganic powder and the polymer in the preparation process of the masterbatch, and promote the mechanical properties and processing properties of the masterbatch; by controlling the ratio of the specific polyether ester and the polycaprolactone polyol and the temperature and time of heat preservation and cooling, the generation of irritating odor in the preparation of the inorganic powder dispersant is well avoided, which is more environmentally friendly; the present invention adds a fluorine-containing polymer auxiliary agent with a specific fluorine content to the dispersant, especially when the fluorine content is 70-75%, the fluidity of the prepared masterbatch can be improved; in addition, the inorganic powder dispersant is used in a low amount, generally 0.5-2% of the total mass. DETAILED DESCRIPTION
[0043] Example 1
[0044] A method for preparing an environmentally friendly inorganic powder dispersant comprises the following steps:
[0045] (1) polyether ester and polycaprolactone polyol are mixed under nitrogen protection, and the mixture is kept at 75° C. for 45 minutes to obtain a mixture A;
[0046] (2) After cooling to 43° C., a fluorine-containing polymer additive was added to the mixture A, and the dispersant was obtained after mixing for 90 minutes.
[0047] The weight ratio of the polyether ester to the polycaprolactone polyol is 1.1:1.
[0048] The polycaprolactone polyol is a polycaprolactone triol with a number average molecular weight of 2000, which was purchased from Hubei Handafei Biotechnology Co., Ltd.
[0049] The weight ratio of the fluorine-containing polymer additive to the polycaprolactone triol is 1:1.6.
[0050] The preparation of the polyether ester comprises: mixing polyether polyol and maleic anhydride, heating to 105° C. and keeping the temperature for 3 hours, discharging, cooling, and grinding to obtain the polyether ester.
[0051] The molar ratio of the polyether polyol to maleic anhydride is 1:1.15.
[0052] The polyether polyol comprises polyethylene glycol and polypropylene glycol in a weight ratio of 1.5:1.
[0053] The polyethylene glycol was purchased from Shanghai Lianji Chemical Co., Ltd., with the model number of PEG800, the number average molecular weight of 720-880, and the hydroxyl value of 127-156 mgKOH / g; the number average molecular weight of the polypropylene glycol was 3000, and the hydroxyl value was 34-42 mgKOH / g.
[0054] The fluorine-containing polymer additive was purchased from Shangxi (Shanghai) Chemical Additive Co., Ltd. The brand is Japan Daikin DA912, and the fluorine content is 70-75%.
[0055] Example 2
[0056] A method for preparing an environmentally friendly inorganic powder dispersant comprises the following steps:
[0057] (1) polyether ester and polycaprolactone polyol are mixed under nitrogen protection, and the mixture is kept at 70° C. for 60 minutes to obtain a mixture A;
[0058] (2) After cooling to 40° C., a fluorine-containing polymer additive was added to the mixture A, and the dispersant was obtained after mixing for 120 minutes.
[0059] The weight ratio of the polyether ester to the polycaprolactone polyol is 0.6:1.
[0060] The polycaprolactone polyol is a polycaprolactone triol with a number average molecular weight of 2000, which was purchased from Hubei Handafei Biotechnology Co., Ltd.
[0061] The weight ratio of the fluorine-containing polymer additive to the polycaprolactone triol is 1:1.4.
[0062] The preparation of the polyether ester comprises: mixing polyether polyol and maleic anhydride, heating to 100° C. and keeping the temperature for 4 hours, discharging, cooling, and grinding to obtain the polyether ester.
[0063] The molar ratio of the polyether polyol to maleic anhydride is 1:1.15.
[0064] The polyether polyol comprises polyethylene glycol and polypropylene glycol in a weight ratio of 1:1.
[0065] The polyethylene glycol was purchased from Shanghai Lianji Chemical Co., Ltd., with the model number of PEG800, the number average molecular weight of 720-880, and the hydroxyl value of 127-156 mgKOH / g; the number average molecular weight of the polypropylene glycol was 3000, and the hydroxyl value was 34-42 mgKOH / g.
[0066] The fluorine-containing polymer additive was purchased from Shangxi (Shanghai) Chemical Additive Co., Ltd. The brand is Japan Daikin DA912, and the fluorine content is 70-75%.
[0067] Example 3
[0068] A method for preparing an environmentally friendly inorganic powder dispersant comprises the following steps:
[0069] (1) polyether ester and polycaprolactone polyol are mixed under nitrogen protection, and the mixture is kept at 80° C. for 30 minutes to obtain a mixture A;
[0070] (2) After cooling to 45° C., a fluorine-containing polymer additive was added to the mixture A, and the dispersant was obtained after mixing for 90 minutes.
[0071] The weight ratio of the polyether ester to the polycaprolactone polyol is 1.5:1.
[0072] The polycaprolactone polyol is a polycaprolactone triol with a number average molecular weight of 2000, which was purchased from Hubei Handafei Biotechnology Co., Ltd.
[0073] The weight ratio of the fluorine-containing polymer additive to the polycaprolactone triol is 1:1.8.
[0074] The preparation of the polyether ester comprises: mixing polyether polyol and maleic anhydride, heating to 120° C. and keeping the temperature for 2 hours, discharging, cooling, and grinding to obtain the polyether ester.
[0075] The molar ratio of the polyether polyol to maleic anhydride is 1:1.15.
[0076] The polyether polyol comprises polyethylene glycol and polypropylene glycol in a weight ratio of 2:1.
[0077] The polyethylene glycol was purchased from Shanghai Lianji Chemical Co., Ltd., with the model number of PEG800, the number average molecular weight of 720-880, and the hydroxyl value of 127-156 mgKOH / g; the number average molecular weight of the polypropylene glycol was 3000, and the hydroxyl value was 34-42 mgKOH / g.
[0078] The fluorine-containing polymer additive was purchased from Shangxi (Shanghai) Chemical Additive Co., Ltd. The brand is Japan Daikin DA912, and the fluorine content is 70-75%.
[0079] Example 4
[0080] This embodiment provides a method for preparing an environmentally friendly inorganic powder dispersant. The specific implementation method is the same as that of Example 1, except that no fluorine-containing polymer additive is added.
[0081] Example 5
[0082] This embodiment provides a method for preparing an environmentally friendly inorganic powder dispersant. The specific implementation method is the same as that of Example 1, except that the mixing time in step (2) is 50 minutes.
[0083] Performance Testing
[0084] The inorganic powder dispersant and carbon black described in Examples 1-5 were added to PET resin, respectively, and mixed, extruded, and granulated to obtain carbon black masterbatch.
[0085] In terms of mass percentage, the carbon black masterbatch comprises 0.6% of inorganic powder additive, 30% of carbon black, and the remainder is PET resin.
[0086] The melt index of the PET resin at 260° C. / 2.16 kg is 14 g / 10 min.
[0087] 1. Melt flow rate
[0088] The melt flow rates of the carbon black masterbatches corresponding to Examples 1-5 were measured according to GB / T3682 standard. The results are shown in Table 1.
[0089] Table 1
[0090] serial number Melt flow rate (g / 10min) Example 1 2.8 Example 2 2.5 Example 3 2.7 Example 4 1.5 Example 5 2.0 Without dispersant 0.3
Claims
1. A method for preparing an environmentally friendly inorganic powder dispersant, characterized in that: At least the following steps are included: (1) Mixing polyether ester and polycaprolactone polyol under nitrogen protection and keeping the mixture warm for a certain period of time to obtain a mixture A; (2) adding a processing aid to the mixture A after cooling, and obtaining the dispersant after mixing; The weight ratio of the polyether ester to the polycaprolactone polyol is (0.6-1.5):1; The polycaprolactone polyol is a polycaprolactone triol; The number average molecular weight of the polycaprolactone triol is 2000; The preparation method of polyether ester comprises: mixing polyether polyol and acid anhydride, heating and keeping the temperature for a period of time, discharging, cooling, and grinding to obtain polyether ester; The polyether polyol comprises polyethylene glycol and polypropylene glycol in a weight ratio of (1-2):1; The polyethylene glycol has a number average molecular weight of 720-880 and a hydroxyl value of 127-156 mgKOH / g; The polypropylene glycol has a number average molecular weight of 3000 and a hydroxyl value of 34-42 mgKOH / g; The anhydride comprises maleic anhydride; The processing aid comprises a fluorine-containing polymer additive, and the fluorine content of the fluorine-containing polymer additive is 65-80%; The weight ratio of the fluorine-containing polymer additive to the polycaprolactone polyol is 1:(1.4-1.8); The mixing time in step (2) is 60-120 minutes.
2. The method for preparing an environmentally friendly inorganic powder dispersant according to claim 1, characterized in that: The insulation temperature in step (1) is 70-80°C.
3. The method for preparing an environmentally friendly inorganic powder dispersant according to claim 1, characterized in that: The insulation time in step (1) is 30-60 minutes.
4. The method for preparing an environmentally friendly inorganic powder dispersant according to claim 1, characterized in that: The cooling temperature in step (2) is 40-50°C.
5. A dispersant prepared by the method for preparing an environmentally friendly inorganic powder dispersant according to any one of claims 1 to 4, which is used for dispersing pigments and fillers in polymers.