A polyurethane composite material with high weather resistance and preparation method thereof

By using polyethylene adipate and MDI as raw materials, adding specific weather-resistant agents, and combining with the injection molding process, the problem of poor weather resistance of thermoplastic polyurethane elastomers has been solved, and applications in wires and cables, automobile sealing strips, and shoe materials have been achieved. It has high weather resistance and excellent mechanical properties in other fields, and is suitable for mass production.

CN115612052BActive Publication Date: 2024-10-25HEFEI GENIUS NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110786306.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-12
Publication Date
2024-10-25
Estimated Expiration
2041-07-12

AI Technical Summary

Technical Problem

The weather resistance of thermoplastic polyurethane elastomer is poor, which limits its application in wires and cables, automobile sealing strips, shoe materials and other fields.

Method used

Using polyethylene adipate and MDI as raw materials, by adding 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazin-4-one and N-( 2-ethylphenyl)-N'-(2-ethoxy-5-tert-butyl)oxalamide is used as a compound weathering agent, combined with the injection molding process, to prepare polyurethane composite materials with high weather resistance.

Benefits of technology

It significantly improves the weather resistance and mechanical properties of polyurethane elastomer, and is suitable for wire and cable, automobile sealing strips, shoe materials and other fields, with simple process and short molding time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003158931080000021
    Figure BDA0003158931080000021
  • Figure BDA0003158931080000031
    Figure BDA0003158931080000031
Patent Text Reader

Abstract

The invention discloses a polyurethane composite material with high weather resistance and a preparation method thereof, wherein the polyurethane composite material is prepared from the following components in parts by weight: 90-110 parts of polyester polyol, 30-35 parts of chain extender, 50-70 parts of MDI, 0.1-1 parts of antioxidant, 0.1-1 parts of dibutyltin dilaurate, 0.5-2 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one, and 0.5-2 parts of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide. The polyurethane elastomer preparation process is simple in the present invention, and the molding time is short. The obtained polyurethane composite material has excellent weather resistance and mechanical properties, and can be widely used in the fields of wires and cables, automotive sealing strips, shoe materials, films, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and particularly relates to a polyurethane composite material with high weather resistance and a preparation method thereof. Background Art

[0002] Thermoplastic polyurethane elastomer, also known as thermoplastic polyurethane rubber, abbreviated as TPU, is a (AB)n type block linear polymer, A is a polyester or polyether with a high molecular weight (1000-6000), B is a diol containing 2-12 straight-chain carbon atoms, and the chemical structure between the AB segments is diisocyanate. Thermoplastic polyurethane rubber relies on intermolecular hydrogen bond crosslinking or mild crosslinking between macromolecular chains. These two crosslinking structures are reversible as the temperature rises or falls. In the molten state or solution state, the intermolecular force is weakened, and after cooling or solvent evaporation, the strong intermolecular force connects together again, restoring the original solid performance.

[0003] Thermoplastic polyurethane elastomer has become one of the important thermoplastic elastomer materials with its excellent performance and wide application. Its molecules are basically linear, with no or little chemical crosslinking. There are many physical crosslinks formed by hydrogen bonds between the molecular chains of linear polyurethane, which strengthen its morphology, thus giving it many excellent properties, such as high modulus, high strength, excellent wear resistance, chemical resistance, hydrolysis resistance, high and low temperature resistance and mildew resistance. These good properties make thermoplastic polyurethane widely used in many fields such as clothing, automotive interior, medicine and health, pipes and sheets. The final product generally does not need to be vulcanized and crosslinked, which can shorten the reaction cycle and reduce energy consumption. Since it is basically a linear structural polymer, it can be processed using the same technology and equipment as thermoplastics, such as injection molding, extrusion, blow molding, calendering, etc., and is particularly suitable for medium and small-sized parts produced in large quantities. Waste materials can be recycled and reused, and different additives or fillers can be used in the production or processing process to improve certain physical properties and reduce costs.

[0004] However, polyurethane elastomers have poor weather resistance. Fields such as wires and cables, automotive sealing strips, shoe materials, and films require high weather resistance. In these fields, the application of polyurethane elastomers is subject to certain restrictions. Summary of the invention

[0005] The purpose of the present invention is to provide a polyurethane composite material with high weather resistance and a preparation method thereof, so as to solve the problems in the prior art.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] A polyurethane composite material with high weather resistance is prepared from the following components in parts by weight:

[0008]

[0009] As a preferred technical solution, the polyester polyol is polyethylene adipate; the polyethylene adipate has a molecular weight of 1000-2500, a hydroxyl value of 60±10 mgKOH / g, an acid value of <2.0 mgKOH / g, and a viscosity of 7000±1000 cpa.s at 25°C; the chain extender is a mixture of 1,4-butanediol and ethylene glycol in a weight ratio of 1:1; and the antioxidant is antioxidant 1135.

[0010] The present invention also provides a method for preparing the polyurethane composite material with high weather resistance, comprising the following steps: 90-110 parts of dehydrated polyester polyol, 30-35 parts of dehydrated chain extender, 50-70 parts of MDI, 0.1-1 parts of dibutyltin dilaurate, 0.1-1 parts of antioxidant, 0.5-2 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one, 0.5-2 parts of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide are mixed uniformly to obtain a mixture, and the mixture is injected into a mold by an injection machine for curing to obtain the target product. Further, the injection temperature of the injection machine is 40-45°C, and the injection pressure is 20-30Mpa; the curing temperature is 90-110°C, and the time is 5-20 minutes.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] The light stability of polyurethane depends largely on the two components of isocyanate and polyol. The present invention specifically selects polyethylene adipate and MDI as raw materials, so that the polymerized polyurethane itself has certain weather resistance.

[0013] Furthermore, the present invention adds 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one and N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide as a composite weathering agent, which can not only reduce the absorption of ultraviolet rays by polyurethane, but also prevent the oxidation reaction of polyurethane macromolecular chains, thereby greatly increasing the weather resistance of the polyurethane elastomer, while maintaining relatively excellent mechanical properties.

[0014] The polyurethane elastomer of the present invention has a simple preparation process and a short molding time, and can be widely used in the fields of electric wires and cables, automobile sealing strips, shoe materials, films, etc. DETAILED DESCRIPTION

[0015] The present invention will be further described below in conjunction with examples. The following examples are merely intended to illustrate the present invention rather than to limit it.

[0016] All raw materials in the examples and comparative examples are commercially available.

[0017] Among them, the chain extender is a mixture of 1,4-butanediol and ethylene glycol in a weight ratio of 1:1; the polyester polyol uses polyethylene adipate with a molecular weight of 2000, a hydroxyl value of 60±10mgKOH / g, an acid value of <2.0mgKOH / g, and a viscosity of 7000±1000cpa.s 25℃; the manufacturers of 1,4-butanediol, ethylene glycol, and polyethylene adipate are Hubei Xinrunde Chemical. MDI is Bayer 44V20 from Germany. The manufacturer of antioxidant 1135 is Condis Chemical. The manufacturers of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one are all American Cytec; the manufacturer of N-(2-ethylphenyl)-N′-(2-ethoxy-5-tert-butylphenyl) oxalamide is Klein Company.

[0018] The material properties of each embodiment and comparative example were tested under the following conditions:

[0019] Tensile strength test: according to ISO 527-2 standard, the sample size is 170*10*4mm, and the tensile speed is 50mm / min;

[0020] Weathering test: The tensile specimens were subjected to UV accelerated aging (UV aging conditions are shown in Table 1) to test their tensile properties.

[0021] Table 1. UV aging conditions

[0022]

[0023] Example 1

[0024] A uniform mixture of 90 parts of dehydrated polyester polyol, 30 parts of dehydrated chain extender, 50 parts of MDI, 0.1 parts of dibutyltin dilaurate, 0.1 parts of antioxidant 1135, 0.5 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one and 0.5 parts of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide was added to an injection machine, and injected into a mold with the injection machine. The injection pressure was 20 MPA, the injection temperature was 40°C, the mold temperature was 90°C, and the mold was demolded after 20 minutes to obtain a finished product.

[0025] Example 2

[0026] A uniform mixture of 110 parts of dehydrated polyester polyol, 35 parts of dehydrated chain extender, 70 parts of MDI, 1 part of dibutyltin dilaurate, 1 part of antioxidant 1135, 2 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one and 2 parts of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl)oxalyl diamide was added into an injection machine, and injected into a mold with the injection machine. The injection pressure was 30 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 5 minutes to obtain a finished product.

[0027] Example 3

[0028] A uniform mixture of 100 parts of dehydrated polyester polyol, 30 parts of dehydrated chain extender, 60 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, 1 part of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one and 1 part of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl)oxalyl diamide was added to an injection machine, and the mixture was injected into a mold with an injection machine. The injection pressure was 25 MPa, the injection temperature was 42°C, the mold temperature was 100°C, and the mold was demolded after 10 minutes to obtain a finished product.

[0029] Example 4

[0030] A uniform mixture of 90 parts of dehydrated polyester polyol, 32 parts of dehydrated chain extender, 65 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, 2 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one and 2 parts of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide was added to an injection machine, and injected into a mold with the injection machine. The injection pressure was 25 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 8 minutes to obtain a finished product.

[0031] Comparative Example 1

[0032] A uniform mixture of 90 parts of dehydrated polyester polyol, 32 parts of dehydrated chain extender, 65 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, and 4 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one was added to an injection machine, and injected into a mold with the injection machine. The injection pressure was 25 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 8 minutes to obtain a finished product.

[0033] Comparative Example 2

[0034] A uniform mixture of 90 parts of dehydrated polyester polyol, 32 parts of dehydrated chain extender, 65 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, and 4 parts of N-(2-ethylphenyl)-N′-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide was added to an injection machine, and injected into a mold using the injection machine. The injection pressure was 25 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 8 minutes to obtain a finished product.

[0035] Comparative Example 3

[0036] A uniform mixture of 90 parts of dehydrated polyester polyol, 32 parts of dehydrated chain extender, 65 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, 2 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one and 2 parts of UV-328 was added to an injection machine and injected into a mold with the injection machine. The injection pressure was 25 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 8 minutes to obtain a finished product.

[0037] Comparative Example 4

[0038] A uniform mixture of 90 parts of dehydrated polyester polyol, 32 parts of dehydrated chain extender, 65 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, 2 parts of UV-9, and 2 parts of N-(2-ethylphenyl)-N′-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide was added to an injection machine, and injected into a mold using the injection machine. The injection pressure was 25 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 8 minutes to obtain a finished product.

[0039] Comparative Example 5

[0040] A uniform mixture of 90 parts of dehydrated polyester polyol, 32 parts of dehydrated chain extender, 65 parts of MDI, 0.5 parts of dibutyltin dilaurate, 0.5 parts of antioxidant 1135, 2 parts of UV-9 and 2 parts of UV-328 was added to an injection machine and injected into a mold with an injection machine. The injection pressure was 25 MPa, the injection temperature was 45°C, the mold temperature was 110°C, and the mold was demolded after 8 minutes to obtain a finished product.

[0041] The physical properties of the products obtained in each embodiment and comparative example were tested, and their properties are shown in Table 2:

[0042] Table 2 Test results of material properties obtained in various embodiments and comparative examples

[0043]

[0044] It can be seen from the results of the above embodiments that the performance of the products prepared in each embodiment is significantly better than that of the products prepared in the comparative examples, indicating that the scheme in the present application can greatly increase the weather resistance of the polyurethane elastomer while maintaining relatively excellent mechanical properties.

[0045] These embodiments are only used to illustrate the present invention and should not limit the scope of the present invention. In addition, after reading the present invention, those skilled in the art will make various equivalent changes or modifications to the present invention, and these equivalents also belong to the scope limited by the claims of the application.

Claims

1. A polyurethane composite material with high weather resistance, characterized in that: It is prepared from the following components in parts by weight:

2. The polyurethane composite material with high weather resistance according to claim 1, characterized in that: The polyester polyol is polyethylene adipate.

3. The polyurethane composite material with high weather resistance according to claim 2, characterized in that: The polyethylene adipate has a molecular weight of 1000-2500, a hydroxyl value of 60±10 mgKOH / g, an acid value of <2.0 mgKOH / g, and a viscosity of 7000±1000 cps at 25°C.

4. The polyurethane composite material with high weather resistance according to claim 1, characterized in that: The chain extender is a mixture of 1,4-butanediol and ethylene glycol in a weight ratio of 1:

1.

5. The polyurethane composite material with high weather resistance according to claim 1, characterized in that: The antioxidant is antioxidant 1135.

6. The method for preparing a polyurethane composite material with high weather resistance according to any one of claims 1 to 5, characterized in that: The following steps are involved: 90-110 parts of dehydrated polyester polyol, 30-35 parts of dehydrated chain extender, 50-70 parts of MDI, 0.1-1 parts of dibutyltin dilaurate, 0.1-1 parts of antioxidant, 0.5-2 parts of 2,2'-(1,4-phenylene)bis-4H-3,1-benzoxazine-4-one, and 0.5-2 parts of N-(2-ethylphenyl)-N'-(2-ethoxy-5-tert-butylphenyl) oxalyl diamide are uniformly mixed to obtain a mixture, and the mixture is injected into a mold by an injection machine for curing to obtain a target product.

7. The method for preparing a polyurethane composite material with high weather resistance according to claim 6, characterized in that: The injection temperature of the injection machine is 40-45°C, and the injection pressure is 20-30Mpa.

8. The method for preparing a polyurethane composite material with high weather resistance according to claim 6, characterized in that: The curing temperature is 90-110° C. and the curing time is 5-20 minutes.