A method for improving roller marks on the surface of ultra-thin steel strip

By controlling multiple parameters of the cast strip and rolls during the twin-roll casting and rolling process, the problem of roll marks during the opening and rolling of ultra-thin strip steel is solved, product quality and production efficiency are improved, and economic losses are reduced.

CN115625199BActive Publication Date: 2024-10-22ZHANGJIAGANG ZHONGMEI UCS TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211185722.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-10-22
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

The existing technology fails to effectively solve the problem of roll marks produced during the rolling process of double-roll cast-rolled ultra-thin strips, resulting in production quality and economic losses.

Method used

By controlling parameters such as thickness, crown, temperature, pre-rolling tension, rolling mill cooling water volume, opening rolling reduction and reduction rate, the design of the casting rolls and rolls is adjusted to ensure the stability of the cast strip during the hot rolling process. and roll surface quality.

Benefits of technology

Significantly reduces the incidence of roll mark defects on the surface of ultra-thin strip steel, improves product quality and qualification rate, and reduces economic losses caused by roll marks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115625199B_ABST
    Figure CN115625199B_ABST
Patent Text Reader

Abstract

The present invention provides a method for improving the roller mark on the surface of ultra-thin strip steel. The method of the present invention at least improves or even avoids the roller mark defects of ultra-thin strip steel produced by twin-roll casting by adjusting parameters such as cast strip thickness, cast strip convexity, cast strip temperature, hot box air flow, pre-rolling tension, rolling mill cooling water volume, rolling mill start-up reduction and reduction rate. The method mainly includes adjusting the cast strip thickness to 1.8-2.0 mm, the cast strip convexity to 35-80 μm, the cast strip temperature to 1050-1200°C, and the hot box air flow to 100-200 m 3 / h, the strip tension before the rolling mill is 2.0-3.5MPa, the rolling reduction is 15-25%, and the rolling reduction rate is 0.6-0.9mm / s. Through one or more of the above measures, the roller mark problem of ultra-thin strip hot rolling can be effectively improved, the roller mark judgment rate can be effectively reduced, and the qualified rate of ultra-thin strip products can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel production, and relates to a plate shape control technology for ultra-thin hot-rolled strip steel, and more specifically to a method for improving roller marks on the surface of ultra-thin strip steel. Background Art

[0002] The ultra-thin strip steel production process of twin-roll thin strip continuous casting is to directly cast the liquid molten steel into a cast strip with a thickness of less than 2.5mm through a pair of casting rolls rotating in opposite directions. The thin cast strip is then sent to the rolling mill rolls through guide rolls and pinch rolls. When the thin strip steel enters the coiler and the coiling tension is established, the rolling mill is pressed down to roll to form an ultra-thin hot-rolled strip steel product. The thickness of the ultra-thin strip steel product is generally less than 1.5mm.

[0003] Due to the extremely thin thickness of the cast strip, the difficulty of hot rolling is greatly increased. During the rolling process of the rolling mill, it is very easy to cause the thin strip steel to be crushed and damage the rolls. In the subsequent rolling process, the surface defects of the rolls are replicated on the surface of the strip, forming continuous roll marks. Usually, such defects last for about 400 tons of products in the entire twin-roll casting production process, forming serious production quality problems.

[0004] At present, domestic research on roller mark problems is mainly concentrated in multi-stand hot rolling, galvanizing process, heat treatment furnace, etc., mainly solving the roller marks caused by the threading process, galvanizing sinking roller marks, and roller marks caused by furnace bottom nodules. None of them involve the roller marks of twin-roll casting and rolling of ultra-thin strip steel. The above methods cannot be used to solve the roller marks caused by the twin-roll casting and rolling process.

[0005] Chinese patent CN103468919B reduces the roller marks on the surface of steel plates by adjusting the temperature gradient in the quenching furnace and the swing speed of the steel plates in the furnace. Chinese patent CN103710518B controls the roller nodules in the heating furnace to notify the roller marks on the surface of steel plates. Both technologies solve the roller marks produced by thick plates during heat treatment. Chinese patents CN106893958B and CN107779803B solve the roller marks on the surface of strip steel during galvanizing production by modifying the automatic spray dust reduction system of the hopper of the galvanizing unit and detecting and modifying the sinking roller. Chinese patent CN110976516B eliminates the roller marks on the surface of multi-pass hot-rolled strip steel by adjusting the descaling water spraying method and increasing the temperature of the strip head. Chinese patent CN112986277B improves the accuracy of roller mark statistics and detection by splicing images captured by the camera, dividing them according to the circumference of the roller, and performing feature matching on sub-blocks at the same position in each divided image. The patent does not propose a method for solving the roller mark problem.

[0006] It can be seen that in the prior art, the solutions to roller marks are all concentrated in the production processes such as hot rolling, galvanizing, and leveling, while no relevant solutions are disclosed for the hot rolling production process of the twin-roll casting process, especially the roller mark problem of the opening rolling. Therefore, it can be said that the solution technology for roller marks on the surface of ultra-thin hot-rolled strip produced by twin-roll casting is still a technical gap in this field. Summary of the invention

[0007] The purpose of the present invention is to provide a production control method for improving or even avoiding roller marks on the surface of ultra-thin strip steel. The method of the present invention controls the convexity, thickness, temperature and surface state of the incoming hot-rolled material, and at the same time controls the pre-rolling tension, rolling mill pressing speed, rolling pressing amount and rolling mill cooling water volume during the hot rolling start-up pressing process, thereby effectively solving the roller mark defects of ultra-thin strip steel generated during the rolling mill pressing process after the hot rolling threading is completed, avoiding the occurrence of batch continuous roller mark defects during the production process of ultra-thin strip steel, and significantly improving the surface quality and product qualification rate of ultra-thin hot-rolled strip steel. At the same time, the method of the present invention also effectively reduces the economic losses caused by surface defects.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] According to a first aspect of the present invention, a method for improving the roll mark on the surface of an ultra-thin steel strip is proposed, the method comprising:

[0010] In the twin-roll casting process:

[0011] (1) The thickness of the cast strip is controlled within the range of 1.8 to 2.0 mm;

[0012] (2) Control the convexity of the cast strip within the range of 35 to 80 μm;

[0013] Before the cast strip enters the hot rolling mill:

[0014] (3) Controlling the casting strip temperature within the range of 1050-1200°C;

[0015] (4) Control the air flow rate of the hot box protective atmosphere at 100-200m 3 / h range;

[0016] (5) Control the strip tension before the rolling mill within the range of 2.0 to 3.5 MPa;

[0017] During the rolling process of the hot rolling mill:

[0018] (6) Control the cooling water volume of the rolling mill within the range of 50-80%;

[0019] (7) Control the rolling reduction within the range of 15% to 25%;

[0020] (8) The rolling speed of the hydraulic cylinder of the rolling mill is controlled within the range of 0.6 to 0.9 mm / s.

[0021] According to the method for improving the roller mark on the surface of ultra-thin strip steel of the present invention, preferably, the step (1) further comprises: adjusting the pressure of the casting roller hydraulic cylinder to control the casting force within the range of 1500 to 4000 N; and / or controlling the casting speed within the range of 40 to 70 m / min to control the thickness of the cast strip within the range of 1.8 to 2.0 mm.

[0022] According to the method for improving the roller mark on the surface of ultra-thin strip steel of the present invention, preferably, the step (2) further comprises: adjusting the surface profile of the casting roll and the convexity of the casting roll to control the convexity of the cast strip plate shape within the range of 40 to 65 μm.

[0023] According to the method for improving the roller mark on the surface of ultra-thin steel strip of the present invention, preferably, the step (3) further comprises: adjusting the nitrogen flow rate in the hot box to 1000-2500m 3 / h to control the temperature of the cast strip before entering the rolling mill in the range of 1050-1150℃.

[0024] According to the method for improving the roller mark on the surface of ultra-thin steel strip of the present invention, preferably, the step (4) further comprises: controlling the air flow rate of the hot box protective atmosphere to 120-160m 3 / h range.

[0025] According to the method for improving the roller mark on the surface of ultra-thin strip steel of the present invention, preferably, the step (4) further comprises: controlling the oxide scale thickness of the cast strip before entering the rolling mill to be in the range of 7 to 13 μm.

[0026] According to the method for improving the roller mark on the surface of ultra-thin steel strip of the present invention, preferably, the step (5) further comprises: controlling the tension of the steel strip before entering the rolling mill to be in the range of 2.0 to 3.0 MPa.

[0027] According to the method for improving the roller mark on the surface of ultra-thin strip steel of the present invention, preferably, the step (6) further comprises: controlling the flow rate of cooling water of the rolling mill, controlling the cooling water volume of the rolling mill within the range of 65-80% to accelerate the establishment of thermal convexity of the rolling mill.

[0028] According to the method for improving the roll mark on the surface of ultra-thin strip steel of the present invention, preferably, the step (7) further comprises: controlling the roll gap of the rolling mill to control the initial rolling reduction within the range of 18% to 25%.

[0029] According to the method for improving the roller mark on the surface of ultra-thin strip steel of the present invention, preferably, the step (8) further comprises: controlling the opening rolling reduction rate of the hot rolling mill to be in the range of 0.7 to 0.85 mm / s.

[0030] According to the method for improving the roller mark on the surface of ultra-thin steel strip of the present invention, preferably, step (7) or step (8) further comprises: adjusting the surface profile of the roller to control the roller crown to 40 to 90 μm.

[0031] According to a second aspect of the present invention, a hot-rolled thin steel strip is provided, wherein the above-mentioned method is used to control the roller mark on the surface of the hot-rolled thin steel strip during the production process.

[0032] According to the hot-rolled thin steel strip of the present invention, preferably, the roll mark failure rate of the hot-rolled ultra-thin steel strip is not higher than 1.0%.

[0033] Beneficial technical effects

[0034] Compared with the prior art, the technical advantages and beneficial technical effects of the present invention include at least:

[0035] The method of the present invention effectively solves the technical problem of roll mark during twin-roll casting by controlling the performance of the ultra-thin cast strip and the parameters of the start rolling reduction. More specifically, the method of the present invention avoids the roll mark defect of the ultra-thin strip produced by twin-roll casting by adjusting parameters such as cast strip thickness, cast strip convexity, cast strip temperature, hot box air flow, pre-rolling tension, rolling mill cooling water volume, rolling mill start rolling reduction and reduction rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly introduce the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings of the embodiments. Obviously, the drawings in the following description only relate to some implementation cases of the present invention, and are not intended to limit the present invention.

[0037] Figure 1 A schematic diagram of roller printing on the surface of ultra-thin steel strip in the prior art is shown;

[0038] Figure 2 A schematic diagram of the surface of the ultra-thin steel strip after being improved by the method of the present invention is shown. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one of ordinary skill in the art to which the present invention belongs.

[0041] When twin-roll casting and rolling is used to produce thin strip steel, the thickness of the cast strip is extremely thin. After entering the hot rolling mill, the hot rolling mill produces compressive stress deformation on the thin strip steel at high temperature during the pressing process, which can easily cause uneven rolling of the wide strip steel along the width direction. The strip steel is severely squeezed locally, causing cracks or waves, causing trauma to the roll surface, and then pressed onto the surface of the hot-rolled thin strip steel again, forming continuous batches of roll marks, such as Figure 1 shown.

[0042] Example 1

[0043] The qualified molten steel is cast into a continuous cast strip through a pair of rotating casting rollers. The casting force is controlled to be 1600N and the casting speed is 65m / min. The cast strip with a thickness of 1.86mm is obtained. According to the adjusted casting roller surface profile, the convexity of the cast strip is controlled to be 58um. After the cast strip is led out of the casting roller, it enters the hot rolling mill through the hot box. Before the roller is pressed down, the nitrogen flow rate in the hot box is adjusted to 1390m3 / h, the temperature of the cast strip before entering the rolling mill is controlled to be 1080℃, the oxygen flow rate in the hot box is adjusted to 150m3 / h, and the oxide scale with a thickness of 10um is formed on the surface of the cast strip before entering the rolling mill. At the same time, the pre-rolling strip tension is adjusted to 2.2MPa. The convexity of the roll is controlled to be 65um through the pre-designed roll profile. During the rolling process, the cooling water volume of the rolling mill is adjusted to 65%, the hydraulic cylinder of the rolling mill is adjusted, the rolling reduction is controlled to be 20%, and the rolling reduction rate is 0.82mm / s. The surface of the ultra-thin steel strip produced by twin-roll casting according to this embodiment is smooth and has no continuous roll mark defects. Figure 2 Further, after the method of Example 1 is improved, the roll printing error rate is 0.6%.

[0044] Example 2

[0045] The qualified molten steel is cast into a continuous cast strip through a pair of rotating casting rollers. The casting force is controlled to be 3800N and the casting speed is 55m / min. The cast strip with a thickness of 1.82mm is obtained. According to the adjusted casting roller surface profile, the convexity of the cast strip is controlled to be 46um. After the cast strip is led out of the casting roller, it enters the hot rolling mill through the hot box. Before the roller is pressed down, the nitrogen flow rate in the hot box is adjusted to 1980m3 / h, the temperature of the cast strip before entering the rolling mill is controlled to be 1105℃, the oxygen flow rate in the hot box is adjusted to 130m3 / h, and the oxide scale with a thickness of 8um is formed on the surface of the cast strip before entering the rolling mill. At the same time, the pre-rolling strip tension is adjusted to 2.9MPa. The convexity of the roll is controlled to be 51um through the pre-designed roll profile. During the rolling process, the cooling water volume of the rolling mill is adjusted to 78%, the hydraulic cylinder of the rolling mill is adjusted, the rolling reduction is controlled to be 24%, and the rolling reduction rate is 0.80mm / s. The surface of the ultra-thin steel strip produced by twin-roll casting according to this embodiment is smooth and has no continuous roll mark defects. After the method of embodiment 2 is improved, the roll mark judgment rate is 0.5%.

[0046] Example 3

[0047] The qualified molten steel is cast into a continuous cast strip through a pair of rotating casting rollers. The casting force is controlled to be 2600N and the casting speed is 48m / min. The cast strip with a thickness of 1.89mm is obtained. According to the adjusted casting roller surface profile, the convexity of the cast strip is controlled to be 62um. After the cast strip is led out of the casting roller, it enters the hot rolling mill through the hot box. Before the roller is pressed down, the nitrogen flow rate in the hot box is adjusted to 2350m3 / h, the temperature of the cast strip before entering the rolling mill is controlled to be 1145℃, the oxygen flow rate in the hot box is adjusted to 155m3 / h, and the oxide scale with a thickness of 12um is formed on the surface of the cast strip before entering the rolling mill. At the same time, the pre-rolling strip tension is adjusted to 2.6MPa. The convexity of the roll is controlled to be 86um through the pre-designed roll profile. During the rolling process, the cooling water volume of the rolling mill is adjusted to 72%, the hydraulic cylinder of the rolling mill is adjusted, the rolling reduction is controlled to be 22%, and the rolling reduction rate is 0.71mm / s. The surface of the ultra-thin steel strip produced by twin-roll casting according to this embodiment is smooth and has no continuous roll mark defects. After the method of embodiment 3 is improved, the roll mark judgment rate is 0.2%.

[0048] The above description is only a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for improving the roller mark on the surface of ultra-thin strip steel, characterized in that: The method comprises the following steps: In the twin-roll casting process: (1) The thickness of the cast strip is controlled within the range of 1.8 to 2.0 mm; (2) Control the convexity of the cast strip within the range of 35 to 80 μm; Before the cast strip enters the hot rolling mill: (3) Controlling the casting strip temperature within the range of 1050-1200°C; (4) Control the air flow rate of the hot box protective atmosphere at 100-200m 3 / h range; (5) Control the strip tension before the rolling mill within the range of 2.0 to 3.5 MPa; During the rolling process of the hot rolling mill: (6) Control the cooling water volume of the rolling mill within the range of 50-80%; (7) Control the rolling reduction within the range of 15% to 25%; (8) The rolling speed of the hydraulic cylinder of the rolling mill is controlled within the range of 0.6 to 0.9 mm / s.

2. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (1) further comprises: Adjust the pressure of the casting roll hydraulic cylinder to control the casting force within the range of 1500 to 4000N; and / or Control the casting speed in the range of 40~70m / min, To control the thickness of the cast strip within the range of 1.8 to 2.0 mm.

3. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (2) further comprises: The surface profile of the casting roll and the convexity of the casting roll are adjusted to control the convexity of the cast strip plate shape within the range of 40 to 65 μm.

4. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (3) further comprises: Adjust the nitrogen flow rate in the hot box to 1000~2500m 3 / h to control the temperature of the cast strip before entering the rolling mill in the range of 1050-1150℃.

5. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (4) further comprises: Control the air flow of the hot box protective atmosphere at 120~160m 3 / h range.

6. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (4) further comprises: The oxide scale thickness of the cast strip before entering the rolling mill is controlled in the range of 7 to 13 μm.

7. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (5) further comprises: The strip tension before entering the rolling mill is controlled in the range of 2.0 to 3.0 MPa.

8. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (6) further comprises: Control the cooling water flow of the rolling mill and keep the cooling water volume of the rolling mill in the range of 65-80% to speed up the establishment of the thermal crown of the roll.

9. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (7) further comprises: The mill roll gap is controlled to keep the initial rolling reduction within the range of 18% to 25%.

10. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 1, characterized in that: The step (8) further comprises: The hot rolling mill's rolling reduction rate is controlled within the range of 0.7 to 0.85 mm / s.

11. The method for improving the roller mark on the surface of ultra-thin steel strip according to claim 9 or 10, characterized in that: The step (7) or step (8) further comprises: Adjust the surface profile of the roller and control the roller crown at 40 to 90 μm.

12. A hot-rolled ultra-thin steel strip, characterized in that: The hot-rolled ultra-thin strip steel is produced by controlling the roller mark using the method according to any one of claims 1 to 11.

13. The hot rolled ultra-thin steel strip according to claim 12, characterized in that: The roll mark failure rate of the hot-rolled ultra-thin strip steel is not higher than 1.0%.