A method for preparing a metal soft magnetic powder pressing die punch
By using high-speed steel powder hot isostatic pressing and forging to prepare metal soft magnetic powder pressing die punches, the problems of insufficient strength and toughness in the existing technology are solved, achieving higher compressive strength and longer service life, while reducing processing costs.
Patent Information
- Application Number
- CN202211285340.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-10-20
AI Technical Summary
The existing metal soft magnetic powder pressing die has low strength and toughness, short service life, high processing cost, and large material loss.
Powdered high-speed steel materials are prepared by hot isostatic pressing of high-speed steel powder. Metal soft magnetic powder is then prepared by forging, quenching, cryogenic treatment and tempering. This process avoids the defects of directly using high-speed steel bars and improves the uniformity and compressive strength of the material.
It improves the compressive strength and toughness of metal soft magnetic powder pressing die punches, extends service life, reduces processing costs, and has the prospect of large-scale industrial application.
Smart Images

Figure CN115625335B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mold processing technology, and in particular to a method for preparing a metal soft magnetic powder pressing die. Background Technology
[0002] A metal soft magnetic powder pressing die is a molding die used to process metal soft magnetic powder into metal soft magnetic powder cores. It mainly consists of a middle die, a core rod (optional, depending on the product structure), and a die punch. To achieve higher density and better magnetic properties in the metal soft magnetic powder core, greater pressure is used for pressing. During pressing, the die punch is subjected to significant pressure, impact, and wear; the die punch must withstand a pressure of 17–23 t / cm² per unit area. 3 This requires that the die-stamping process be carried out using materials that combine high strength, good toughness, excellent fatigue resistance and wear resistance.
[0003] Metal soft magnetic powder pressing die punches are generally made of ordinary high-speed steel bars that are directly machined. The machining process involves a large amount of turning, resulting in significant material loss and labor time, thus increasing the processing cost of the die punches. Furthermore, ordinary high-speed steel has defects such as coarse eutectic carbides, carbide segregation, and anisotropy in material properties, which reduce the material's strength, toughness, and wear resistance. Die punches made from ordinary high-speed steel have a short service life, further increasing the cost of using the die.
[0004] CN107442721A discloses a hot forging process for a mold, which includes the following steps: blanking: preparing Cr12 steel bars; billet preparation: removing oxide scale and microcracks from the surface of the bars to obtain a bar-shaped billet with a high-quality surface; pre-forging heat treatment: heating the bar-shaped billet in a heating furnace to remove its stress; forging: forging the bar-shaped billet using hot forging equipment to obtain a mold with a predetermined shape; quenching: quenching the mold in a quenching furnace at a quenching oil temperature of 1080-1150℃ for 10-15 minutes; first tempering: heating the mold to 480-500℃ in a heating furnace and holding it at that temperature for 2-2.5 hours, then removing it from the furnace and allowing it to cool naturally; cryogenic treatment: cooling the mold to ~198℃ using a cooling device and holding it at that temperature for 2-2.5 hours; second tempering: heating the mold to 400℃ and holding it at that temperature for 24 hours, then removing it from the furnace and allowing it to cool naturally.
[0005] CN113997026A discloses a corrosion-resistant mold manufacturing method, including the following steps: S1: mold design; S2: material selection and processing; S3: mold inspection; S4: trial molding; S5: nitriding; A corrosion-resistant mold manufacturing method includes the following steps: S1: main material ratio; S2: heat treatment; S3: wire cutting; S4: electrical discharge machining; S5: mold polishing. The mold undergoes preheating, quenching, deep cooling, and tempering treatments. Compared to other quenching methods, this method effectively improves the mold's hardness. Setting fixing parts before wire cutting and filling the gaps with hot melt adhesive effectively prevents mold deformation and avoids positional displacement during wire cutting, improving the accuracy of mold production. By placing the metal mold in an anti-corrosion solvent for ultrasonic cleaning before polishing and then polishing its surface after low-temperature storage, the polishing difficulty is reduced, and the mold's corrosion resistance is greatly improved.
[0006] CN101670437A discloses a mold manufacturing method with conformal cooling channels. The technical solution involves manufacturing a mold outer contour shell with a designed wall thickness using laser melting forming. Conformal cooling channels are then fabricated and installed within the mold outer contour shell. The mold outer contour shell is preheated, and the gap between the mold cooling channels and the mold outer contour shell is filled by casting. Finally, the mold outer contour shell and the cast-in-place portion undergo overall surface finishing. This mold manufacturing method is simple, has high mold manufacturing precision, and allows the mold cooling channels to be arbitrarily set according to design requirements, meeting the cooling requirements of the mold during use and improving its service life. It also reduces mold manufacturing costs and cycle time, and can meet different mold manufacturing needs by changing the material of the mold outer contour shell.
[0007] However, the molds obtained by the above methods have low strength and toughness, and are not very effective when used to press soft magnetic metal powder.
[0008] Therefore, it is of great significance to develop a method for preparing a metal soft magnetic powder pressing die with high strength, good toughness and good service life. Summary of the Invention
[0009] In view of the problems existing in the prior art, the present invention provides a method for preparing a metal soft magnetic powder pressing die stamp. The method uses high-speed steel powder obtained by hot isostatic pressing as raw material, and then performs forging to prepare the finished metal soft magnetic powder pressing die stamp. Compared with the prior art of directly forging pressing dies from high-speed steel bars, the finished product has better strength, toughness, wear resistance, and service life. Compared with the prior art of directly machining pressing dies from high-speed steel bars, it saves raw materials and reduces manufacturing costs, while also providing better strength, toughness, wear resistance, and a longer service life.
[0010] To achieve this objective, the present invention adopts the following technical solution:
[0011] This invention provides a method for preparing a metal soft magnetic powder pressing die, the method comprising the following steps:
[0012] (1) The high-speed steel powder obtained by vacuum atomization powdering is loaded into a package, and after vacuuming, it is subjected to hot isostatic pressing to obtain powdered high-speed steel material.
[0013] (2) The powdered high-speed steel material is forged to form a metal soft magnetic powder pressing die blank;
[0014] (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching, deep cryogenic treatment, tempering and fine machining in sequence to obtain the finished metal soft magnetic powder pressing die.
[0015] The method for preparing the metal soft magnetic powder pressing die punch of this invention employs a forging process using powdered high-speed steel. This method saves significant amounts of material, reduces machining labor and tool wear costs, and lowers the overall processing cost of the die punch. Furthermore, the resulting die punch exhibits higher compressive strength and better toughness along the streamline direction, resulting in a longer service life and meeting the requirements for pressing metal soft magnetic powder. In this invention, high-speed steel powder is encased in a sleeve and subjected to hot isostatic pressing followed by forging. Due to the protective effect of the sleeve, the powdered high-speed steel material does not suffer from decarburization or element loss. Moreover, the powdered high-speed steel material has a uniform microstructure, free from coarse carbides and segregation, significantly reducing the forging difficulty. The preparation process is easily controlled, and the resulting metal soft magnetic powder pressing die punch has a long service life, demonstrating promising prospects for large-scale industrial application.
[0016] The high-speed steel described in this invention is a well-known technical term in the field. It is a tool steel with high hardness, high wear resistance, and high heat resistance, also known as high-speed tool steel or high-speed steel, and commonly referred to as white steel. Powder high-speed steel refers to high-speed steel obtained by producing a dense steel billet using powder metallurgy methods, followed by hot deformation such as forging and rolling.
[0017] Preferably, the high-speed steel powder in step (1) includes any one of HPM20, HPM23 or HPM05.
[0018] Preferably, the oxygen content of the high-speed steel powder in step (1) is ≤200ppm, for example, it can be 200ppm, 190ppm, 180ppm, 150ppm, 130ppm or 100ppm, etc., but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0019] Preferably, the proportion of powder with a particle size of less than 90 μm in the high-speed steel powder is more than 90%, such as 90%, 92%, 94%, 95%, 97% or 99%, etc., but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0020] Preferably, the material of the sleeve in step (1) includes low-carbon steel plate or strip.
[0021] Preferably, the wall thickness of the sleeve in step (1) is 2 to 5 mm, for example, it can be 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm or 5 mm, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0022] Preferably, the vacuum level inside the enclosure after vacuuming is ≤9×10⁻⁶. -2 Pa, for example, could be 9 × 10 -2 Pa, 2×10 -2 Pa, 9×10 -3 Pa, 7×10 -3 Pa, 5×10 -3 Pa, 3×10 -3 Pa or 1×10 -3 Pa, etc., but not limited to the listed values; other unlisted values within this range also apply.
[0023] Preferably, the temperature of the hot isostatic pressing process in step (1) is 1100 to 1180°C, for example, it can be 1100°C, 1105°C, 1120°C, 1140°C, 1160°C or 1180°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0024] Preferably, the pressure of the hot isostatic pressing treatment is 100-200 MPa, for example, it can be 100 MPa, 120 MPa, 140 MPa, 150 MPa, 180 MPa or 200 MPa, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0025] Preferably, the initial forging temperature of the forging process in step (2) is 1100 to 1180°C, for example, it can be 1100°C, 1105°C, 1120°C, 1140°C, 1160°C or 1180°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0026] The preferred forging temperature of the forging process in this invention is 1100-1180℃. When the initial forging temperature is too low, forging cannot be performed, or the die-stamped blank is prone to cracking during the forging process. When the initial forging temperature is too high, the powder high-speed steel material will overheat or burn, and it is prone to cracking during the forging process, and the resulting die-stamped blank has poor strength and toughness.
[0027] Preferably, the final forging temperature of the forging process is 900-950℃, for example, it can be 900℃, 910℃, 920℃, 930℃ or 950℃, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0028] Preferably, the quenching temperature in step (3) is 1050 to 1200°C, for example, it can be 1050°C, 1060°C, 1070°C, 1100°C, 1150°C or 1200°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0029] Preferably, the quenching is followed by oil cooling or high-pressure gas cooling.
[0030] Preferably, the pressure of the high-pressure gas cooling is 6 bar or higher, such as 6 bar, 7 bar, 8 bar, 9 bar, 10 bar, or 15 bar, but is not limited to the listed values; other unlisted values within this range are also applicable. Preferably, the cryogenic treatment includes placing the oil-cooled or high-pressure gas-cooled metal soft magnetic powder into a cryogenic treatment furnace and cooling it to -60°C to -190°C, such as -60°C, -80°C, -100°C, -130°C, -150°C, or -190°C, but is not limited to the listed values; other unlisted values within this range are also applicable.
[0031] Preferably, the tempering temperature in step (3) is 560 to 600°C, for example, it can be 560°C, 570°C, 580°C, 590°C or 600°C, but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0032] Preferably, the tempering is performed three times, and after each tempering, the temperature is cooled to below 30°C, for example, 30°C, 28°C, 25°C, 22°C or 20°C, etc., but it is not limited to the listed values. Other unlisted values within this range are also applicable.
[0033] As a preferred technical solution of the present invention, the preparation method includes the following steps:
[0034] (1) High-speed steel powder with an oxygen content of ≤200ppm obtained by vacuum atomization is packed into a sleeve with a wall thickness of 2-5mm, and after vacuuming, it is subjected to hot isostatic pressing at a temperature of 1100-1180℃ and a pressure of 100-200MPa to obtain powdered high-speed steel material.
[0035] The high-speed steel powder contains more than 90% powder particles with a diameter of less than 90 μm; the sheath is made of low-carbon steel plate or strip; the vacuum degree inside the sheath after vacuuming is ≤9×10⁻⁶. -2 Pa;
[0036] (2) The powdered high-speed steel material is forged at an initial forging temperature of 1100-1180℃ and a final forging temperature of 900-950℃ to produce a metal soft magnetic powder pressing die blank.
[0037] (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching at a temperature of 1050-1200℃, deep cryogenic treatment, tempering at a temperature of 560-600℃ three times, and fine machining to obtain the finished metal soft magnetic powder pressing die blank.
[0038] The quenching process involves oil cooling or high-pressure gas cooling; the pressure of the high-pressure gas cooling is above 6 bar; the cryogenic treatment includes pressing the oil-cooled or high-pressure gas-cooled soft magnetic metal powder into a cryogenic treatment furnace and cooling it to -60℃ to -190℃; after each tempering, the temperature is cooled to below 30℃.
[0039] Compared with the prior art, the present invention has at least the following beneficial effects:
[0040] (1) In the preparation method of the metal soft magnetic powder pressing die provided by the present invention, the powder high-speed steel material obtained by hot isostatic pressing of high-speed steel powder has a uniform structure, no carbide segregation, and its compressive strength, impact toughness and wear resistance are all better than ordinary high-speed steel bar material. The service life of the final metal soft magnetic powder pressing die is more than 3 times that of ordinary high-speed steel die.
[0041] (2) The preparation method of metal soft magnetic powder pressing die provided by the present invention greatly reduces the forging difficulty of powder high-speed steel material, has low processing cost, and has the prospect of large-scale industrial application. Attached Figure Description
[0042] Figure 1 This is a metallographic image of the HPM20 high-speed steel powder in Example 1.
[0043] Figure 2 This is the metallographic diagram of the M2 high-speed steel bar in Comparative Example 2. Detailed Implementation
[0044] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0045] The present invention will now be described in further detail. However, the examples described below are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention is determined by the claims.
[0046] Example 1
[0047] This embodiment provides a method for preparing a metal soft magnetic powder pressing die, the method comprising the following steps:
[0048] (1) HPM20 high-speed steel powder with an oxygen content of 200 ppm obtained by vacuum atomization was packed into a low-carbon steel plate sleeve with a wall thickness of 3 mm. After vacuuming, it was subjected to hot isostatic pressing at a temperature of 1100℃ and a pressure of 150 MPa to obtain powdered high-speed steel material; the metallographic image of HPM20 high-speed steel powder is shown below. Figure 1 As shown;
[0049] The high-speed steel powder contains 93% powder particles with a diameter of less than 90 μm; the vacuum level inside the casing after vacuuming is 2 × 10⁻⁶. -2 Pa;
[0050] (2) The powdered high-speed steel material is forged at an initial forging temperature of 1180℃ and a final forging temperature of 950℃ to form a metal soft magnetic powder pressing die blank.
[0051] (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching at 1200℃, deep cryogenic treatment, tempering at 560℃ three times, and fine machining to obtain the finished metal soft magnetic powder pressing die blank.
[0052] The quenching is followed by oil cooling; the cryogenic treatment includes pressing the oil-cooled soft magnetic metal powder into a cryogenic treatment furnace and cooling it to -60°C; and cooling it to 20°C after each tempering.
[0053] Example 2
[0054] This embodiment provides a method for preparing a metal soft magnetic powder pressing die, the method comprising the following steps:
[0055] (1) The high-speed steel powder with an oxygen content of 180ppm obtained by vacuum atomization was packed into a strip with a wall thickness of 2mm. After vacuuming, it was subjected to hot isostatic pressing at a temperature of 1180℃ and a pressure of 100MPa to obtain powdered high-speed steel material.
[0056] The high-speed steel powder contains 94% powder particles with a diameter of less than 90 μm; the vacuum level inside the casing after vacuuming is 5 × 10⁻⁶. -3 Pa;
[0057] (2) The powdered high-speed steel material is forged at an initial forging temperature of 1140℃ and a final forging temperature of 900℃ to form a metal soft magnetic powder pressing die blank.
[0058] (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching at 1150℃, deep cryogenic treatment, tempering at 600℃ three times, and fine machining to obtain the finished metal soft magnetic powder pressing die blank.
[0059] The quenching is followed by high-pressure air cooling; the pressure of the high-pressure air cooling is 7 bar; the cryogenic treatment includes pressing the high-pressure air-cooled metal soft magnetic powder into a die and placing it into a cryogenic treatment furnace to cool to -190°C; and cooling to 25°C after each tempering.
[0060] Example 3
[0061] This embodiment provides a method for preparing a metal soft magnetic powder pressing die, the method comprising the following steps:
[0062] (1) The high-speed steel powder with an oxygen content of 120ppm obtained by vacuum atomization powdering is packed into a low carbon steel plate with a wall thickness of 5mm. After vacuuming, it is subjected to hot isostatic pressing at a temperature of 1140℃ and a pressure of 200MPa to obtain powdered high-speed steel material.
[0063] The high-speed steel powder contains 91% powder particles with a diameter of less than 90 μm; the vacuum level inside the casing after vacuuming is 7 × 10⁻⁶. -3 Pa;
[0064] (2) The powdered high-speed steel material is forged at an initial forging temperature of 1100℃ and a final forging temperature of 930℃ to form a metal soft magnetic powder pressing die blank.
[0065] (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching at 1100℃, deep cryogenic treatment, tempering at 570℃ three times, and fine machining to obtain the finished metal soft magnetic powder pressing die blank.
[0066] The quenching process involves high-pressure air cooling to 25°C; the pressure of the high-pressure air cooling is 6 bar; the cryogenic treatment includes pressing the high-pressure air-cooled metal soft magnetic powder into a cryogenic treatment furnace and cooling it to -100°C; and cooling it to 25°C after each tempering.
[0067] Comparative Example 1
[0068] This comparative example provides a method for preparing a metal soft magnetic powder pressing die. The preparation method is the same as in Example 1, except that the HPM20 high-speed steel powder in step (1) is replaced with DC53 powder.
[0069] In this comparative example, DC53 powder has the disadvantages of low compressive strength and poor wear resistance compared with high-speed steel powder. Therefore, the service life of the metal soft magnetic powder pressing die obtained is 1:6 compared with the service life of the metal soft magnetic powder pressing die obtained in Example 1.
[0070] Comparative Example 2
[0071] This comparative example provides a method for preparing a metal soft magnetic powder pressing die, the method comprising the following steps:
[0072] (1) M2 high-speed steel bar material is forged at an initial forging temperature of 1180℃ and a final forging temperature of 950℃ to produce a metal soft magnetic powder pressing die blank.
[0073] (2) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching at 1150℃, deep cryogenic treatment, tempering at 560℃ three times, and fine machining to obtain the finished metal soft magnetic powder pressing die blank.
[0074] After quenching, the material is oil-cooled; after each tempering, it is cooled to 20°C.
[0075] The metallographic diagram of the M2 high-speed steel bar in this comparative example is as follows: Figure 2 As shown, the M2 high-speed steel bar has defects such as coarse eutectic carbides, carbide segregation, and anisotropy of material properties. Therefore, the service life of the metal soft magnetic powder pressing die obtained is 1:3 compared with that of the metal soft magnetic powder pressing die obtained in Example 1.
[0076] Comparative Example 3
[0077] This comparative example provides a method for preparing a metal soft magnetic powder pressing die punch, the method comprising: machining an M2 high-speed steel bar to obtain a finished metal soft magnetic powder pressing die punch.
[0078] In this comparative example, the turning process of the M2 high-speed steel bar involves a large cutting amount, resulting in a significant waste of raw materials, a substantial amount of machining time, and significant wear on the cutting tools. This also leads to high costs in preparing the metal soft magnetic powder pressing die. Furthermore, the service life of the prepared metal soft magnetic powder pressing die is 1:4 that of the die obtained in Example 1.
[0079] The results of the compressive strength, impact toughness, wear volume per unit time, and service life of the metal soft magnetic powder pressing die blanks obtained in the above embodiments are shown in Table 1.
[0080] Table 1
[0081]
[0082] As shown in Table 1, the compressive strength of the metal soft magnetic powder pressed die blanks obtained in Examples 1-3 can reach 3950 MPa, the impact toughness can reach 62 J, and the wear volume per unit time is only 1.1 × 10⁻⁶. -4 cm 3 The final product, made by pressing metal soft magnetic powder into a die, has a service life of up to 550,000 cycles.
[0083] Moreover, the preparation method of the metal soft magnetic powder pressing die punch of the present invention greatly reduces the forging difficulty of the powder high-speed steel material, has low processing cost, and has the prospect of large-scale industrial application.
[0084] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a metal soft magnetic powder pressing die punch to improve compressive strength and impact toughness, characterized in that, The preparation method includes the following steps: (1) High-speed steel powder obtained by vacuum atomization is loaded into a casing, vacuumed, and then subjected to hot isostatic pressing to obtain powdered high-speed steel material; the oxygen content of the high-speed steel powder is ≤200ppm; the proportion of powder with a particle size of less than 90μm in the high-speed steel powder is more than 90%; the casing material includes low-carbon steel plate or strip; the wall thickness of the casing is 2~5mm; the vacuum degree inside the casing after vacuuming is ≤9×10 -2 Pa; The obtained powdered high-speed steel material has a uniform microstructure and no carbide segregation; (2) The powdered high-speed steel material is forged to form a metal soft magnetic powder pressing die blank; (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching, deep cryogenic treatment, tempering and fine machining in sequence to obtain the finished metal soft magnetic powder pressing die blank; The quenching process involves oil cooling or high-pressure gas cooling, and the cryogenic treatment includes pressing the oil-cooled or high-pressure gas-cooled soft magnetic metal powder into a cryogenic treatment furnace and cooling it to -60℃ to -150℃; the tempering process is performed three times.
2. The preparation method according to claim 1, characterized in that, The temperature of the hot isostatic pressing process in step (1) is 1100~1180℃.
3. The preparation method according to claim 1, characterized in that, The pressure for the hot isostatic pressing process is 100~200MPa.
4. The preparation method according to claim 1, characterized in that, The initial forging temperature of the forging process in step (2) is 1100~1180℃.
5. The preparation method according to claim 1, characterized in that, The final forging temperature of the forging process is 900~950℃.
6. The preparation method according to claim 1, characterized in that, The quenching temperature in step (3) is 1050~1200℃.
7. The preparation method according to claim 1, characterized in that, The pressure of the high-pressure air cooler is above 6 bar.
8. The preparation method according to claim 1, characterized in that, The tempering temperature in step (3) is 560~600℃.
9. The preparation method according to claim 1, characterized in that, After each tempering, cool to below 30°C.
10. The preparation method according to claim 1, characterized in that, The preparation method includes the following steps: (1) High-speed steel powder with an oxygen content of ≤200ppm obtained by vacuum atomization is packed into a sleeve with a wall thickness of 2~5mm, and after vacuuming, it is subjected to hot isostatic pressing at a temperature of 1100~1180℃ and a pressure of 100~200MPa to obtain powdered high-speed steel material. The high-speed steel powder contains more than 90% powder with a particle size of less than 90μm; the sheath is made of low-carbon steel plate or strip; the vacuum degree inside the sheath after vacuuming is ≤9×10⁻⁶. -2 Pa; (2) The powdered high-speed steel material is forged at an initial forging temperature of 1100~1180℃ and a final forging temperature of 900~950℃ to form a metal soft magnetic powder pressing die blank. (3) The metal soft magnetic powder pressing die blank is subjected to rough machining, quenching at a temperature of 1050~1200℃, deep cryogenic treatment, tempering at a temperature of 560~600℃ three times and fine machining to obtain the finished metal soft magnetic powder pressing die blank. The quenching is followed by oil cooling or high-pressure gas cooling; the pressure of the high-pressure gas cooling is above 6 bar; the cryogenic treatment includes pressing the oil-cooled or high-pressure gas-cooled soft magnetic metal powder into a cryogenic treatment furnace and cooling it to -60℃ to -150℃; after each tempering, it is cooled to below 30℃.
Citation Information
Patent Citations
Mould making method with conformal cooling pipe
CN101670437A
Hot forging process of mould
CN107442721A
Manufacturing method for corrosion-resistant mold
CN113997026A
High-hardness high-wear-resistant powder metallurgy high-speed steel
CN101586214A
Powder steel and preparation method thereof
CN111118383A