A solid luminescent material and its preparation method and application
By dispersing A2XF6:Mn4+ phosphor particles into SiO2 aerogel and surface modification, a superhydrophobic phosphor-aerogel composite material is formed, which solves the stability of phosphor in a water environment and extends the The service life is maintained and the high luminous efficiency is maintained.
Patent Information
- Application Number
- CN202211302970.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-10-24
AI Technical Summary
The luminescence efficiency of existing phosphors decreases when encountering polar water molecules in the air, and the service life is short. The commonly used coating methods cannot effectively isolate water erosion for a long time, and high-temperature preparation methods will damage the luminescence performance of the phosphors.
The A2XF6:Mn4+ phosphor particles are evenly dispersed into the SiO2 aerogel, and the SiO2 aerogel is hydrophobic through surface modification to form a superhydrophobic phosphor-aerogel composite luminescent material, and prepared at low temperature to maintain fluorescence The stability of the powder.
It effectively improves the problem of phosphor failure when encountering water or water vapor, extends the service life of related devices, and maintains the high luminous efficiency of phosphor.
Smart Images

Figure CN115637145B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of fluorescent materials, and in particular to a solid luminescent material and a preparation method and application thereof. Background Art
[0002] Phosphor A2XF6:Mn 4+ , namely Mn 4+ The emission peak of doped fluoride A2XF6 (A = Na, K, Rb, Cs; X = Si, Ge, Sn, Ti, Zr) under blue light excitation is around 630nm, and it has the advantages of narrow half-width and high emission efficiency. It has practical application needs in the fields of white light LED, plant lighting, high color gamut display, etc. Due to the characteristics of ionic crystals of fluorescent materials, polar water molecules in the air can cause the phosphor to deteriorate, resulting in a decrease in its luminous efficiency and a shortened service life of the lamp. The commonly used method to improve the water erosion resistance of phosphors is surface coating, such as C coating, CaF2 coating, oleic acid and other organic coating, etc., but these coating methods cannot effectively isolate water erosion for a long time, so new coating methods need to be developed.
[0003] Chinese patent CN113717718A discloses a Tb-doped Al2O3 aerogel green phosphor, which uses Al2O3 aerogel to coat the phosphor. Although Al2O3 aerogel can stably coat the phosphor, its preparation temperature is as high as 750°C, and the preparation method cannot ensure the hydrophobicity of the phosphor surface. Moreover, the high temperature used in the preparation method will make the phosphor's luminescence performance ineffective, and it cannot be used for performance optimization and modification of the phosphor. Summary of the invention
[0004] The purpose of the embodiment of the present application is to provide a solid luminescent material and a preparation method and application thereof. 4+ The phosphor particles are evenly dispersed in the SiO2 aerogel, and the SiO2 aerogel is surface-modified to obtain a super-hydrophobic phosphor-aerogel composite luminescent material. The preparation temperature is low, and the problem of phosphor failure when exposed to water or water vapor can be effectively solved, thereby improving the stability and life of related devices.
[0005] In a first aspect, the present invention provides a solid luminescent material, which includes SiO2 aerogel and phosphor A2XF6:Mn dispersed in the SiO2 aerogel. 4+ , the surface of SiO2 aerogel is also grafted with hydrophobic groups.
[0006] In the above technical solution, since SiO2 aerogel is amorphous, has a low formation temperature, and has porous properties and surface hydrophobic modification properties, A2XF6:Mn 4+The phosphor particles are evenly dispersed in the pores of the SiO2 aerogel, and hydrophobic groups are grafted on the surface of the SiO2 aerogel, thereby obtaining a super-hydrophobic phosphor-aerogel composite luminescent material, which effectively solves the problem of fluoride red powder failing when exposed to water or water vapor, and improves the stability and life of related devices.
[0007] In a possible implementation, the particle size of the phosphor is 0.01-30 μm.
[0008] In the above technical solution, the phosphor particles can emit red fluorescence under the excitation of blue light.
[0009] In a possible implementation, the SiO2 aerogel has a porous structure with a pore size of 1 to 100 nm and a porosity of >99%.
[0010] In the above technical solution, SiO2 aerogel is a porous structure, has no photofluorescence, and has low absorption rate and high transmittance to visible light.
[0011] In a possible implementation, the SiO2 aerogel is in the form of powder, block or film.
[0012] In the above technical solution, the solid luminescent material has various structural forms and is widely used.
[0013] In a second aspect, an embodiment of the present application provides a method for preparing the solid light-emitting material provided in the first aspect, comprising the following steps:
[0014] SiO2 sol and phosphor A2XF6:Mn 4+ Mix well, and then gel the SiO2 sol to obtain the dispersed phosphor A2XF6:Mn 4+ SiO2 wet gel;
[0015] The SiO2 wet gel was surface modified to graft hydrophobic groups and then dried to obtain a dispersed phosphor A2XF6:Mn 4+ SiO2 aerogel.
[0016] In the above technical solution, since SiO2 aerogel is amorphous and has a low formation temperature, in the process of forming SiO2 gel, A2XF6:Mn 4+ The phosphor particles are evenly dispersed in the pores of the SiO2 wet gel, and the SiO2 aerogel surface is modified and dried to obtain a super-hydrophobic phosphor-aerogel composite luminescent material. The preparation temperature is low and the obtained solid luminescent material can maintain long-term stability.
[0017] In a possible implementation, the preparation method of SiO2 sol is: dissolving the component raw materials for forming SiO2 aerogel in a solvent, adding a hydrolysis catalyst, stirring, and standing to obtain SiO2 sol.
[0018] In a possible implementation, the preparation method of SiO2 aerogel is as follows: in a dispersion containing phosphor A2XF6:Mn 4+ Add a polycondensation catalyst to the SiO2 sol and stir evenly. The SiO2 sol gradually solidifies into a wet gel. Then add an aging liquid to replace the liquid therein and let it stand for aging.
[0019] In a possible implementation, the surface modification method is: immersing the SiO2 wet gel in a solution containing a surface modifier.
[0020] In one possible implementation, after the surface modification, the pores of the SiO2 wet gel are first filled with a solvent, and then CO2 supercritical drying is performed.
[0021] In a third aspect, an embodiment of the present application provides an application of the solid light-emitting material provided in the first aspect in a white light LED, a white light LD, a plant lighting lamp or a display device. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 A schematic diagram of the structure of a solid light-emitting material provided in an embodiment of the present application;
[0024] Figure 2 A flow chart for preparing a solid luminescent material provided in an embodiment of the present application;
[0025] Figure 3 Schematic diagram of the hydrophobicity of the raw phosphor and the coated phosphor in Example 1;
[0026] Figure 4 K2SiF6:Mn of Example 1 4+ -XRD pattern of SiO2 aerogel red light composite phosphor;
[0027] Figure 5 K2SiF6:Mn of Example 1 4+ -Excitation-emission spectrum of SiO2 aerogel red light composite phosphor;
[0028] Figure 6 K2SiF6:Mn of Example 2 4+ -Photos of SiO2 aerogel blocks under different light irradiation;
[0029] Figure 7 K2SiF6:Mn of Example 3 4+ Electroluminescence spectrum of LED light source made of red and green composite phosphor of / β-sialon-SiO2 aerogel;
[0030] Figure 8 K2SiF6:Mn of Example 3 4+ Chromaticity diagram of LED light source made of red and green composite phosphor of / β-sialon-SiO2 aerogel;
[0031] Fig. 9 K2TiF6:Mn of Example 4 4+ -Excitation-emission spectrum of SiO2 aerogel red light composite phosphor;
[0032] Fig.10 K2GeF6:Mn of Example 5 4+ -Excitation-emission spectrum of SiO2 aerogel red light composite phosphor. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0034] The solid light-emitting material and its preparation method and application in the embodiments of the present application are described in detail below.
[0035] Please see Figure 1 The embodiment of the present application provides a solid luminescent material, which includes SiO2 aerogel and phosphor A2XF6:Mn dispersed in the SiO2 aerogel. 4+ , the surface of SiO2 aerogel is also grafted with hydrophobic groups.
[0036] Among them, SiO2 aerogel is in powder, block or film form; SiO2 aerogel has a porous structure, the pore size is 1 to 100nm, the porosity is >99%, and SiO2 aerogel is amorphous. Phosphor A2XF6:Mn 4+ , namely Mn 4+Doped fluoride A2XF6 (A = Na, K, Rb, Cs; X = Si, Ge, Sn, Ti, Zr), phosphor A2XF6:Mn 4+ The particle size is 0.01-30μm.
[0037] From the perspective of the solid luminescent material as a whole, it is in the form of powder, block or film. Some pores of SiO2 aerogel are filled with phosphor particles, while some are not filled and appear as pores. In the entire solid luminescent material, the mass content of phosphor is usually between 0 and 80%, that is, 0 < phosphor content < 80%.
[0038] The present invention also provides a method for preparing the above-mentioned solid luminescent material, which comprises the following steps:
[0039] SiO2 sol and phosphor A2XF6:Mn 4+ Mix well, and then gel the SiO2 sol to obtain the dispersed phosphor A2XF6:Mn 4+ SiO2 wet gel.
[0040] The SiO2 wet gel was surface modified to graft hydrophobic groups and then dried to obtain a dispersed phosphor A2XF6:Mn 4+ SiO2 aerogel.
[0041] As an implementation method, see Figure 2 , the specific process is:
[0042] S1. Dissolve the component raw materials used for hydrolysis to form SiO2 (such as ethyl orthosilicate, water glass Na2SiO3, tetramethoxysilane, etc.) in a solvent (such as ethanol, ethanol aqueous solution, etc.), add a hydrolysis catalyst (such as oxalic acid, hydrochloric acid, etc.), stir and let stand for a period of time to obtain SiO2 sol.
[0043] S2. Add a certain amount of phosphor A2XF6:Mn into the SiO2 sol 4+ , stirring and mixing evenly to obtain a dispersed phosphor A2XF6:Mn 4+ of SiO2 sol.
[0044] S3, dispersed with phosphor A2XF6:Mn 4+ Add a polycondensation catalyst (such as ammonia water, etc.) to the SiO2 sol, stir evenly, and the SiO2 sol gradually solidifies into a gel; then add an aging liquid (such as ethanol) to replace the liquid in it, let it stand for aging, and obtain a dispersed A2XF6:Mn 4+ SiO2 wet gel.
[0045] S4, soaking the formed SiO2 wet gel in a solution containing a surface modifier (such as hexamethyldisilazane, trimethylchlorosilane, etc.), and then drying to obtain a surface-modified SiO2 wet gel embedded with phosphor A2XF6:Mn 4+ SiO2 sol (phosphor-aerogel composite material), that is, solid luminescent material.
[0046] In the above process, the porosity of the generated SiO2 aerogel is very large, above 99%, and the pore size is generally nanometer-sized. Although the phosphor particles are larger in size, micrometers, this does not prevent the pores of the SiO2 aerogel from accommodating the phosphor particles. This is mainly because a spatial network structure is formed during the SiO2 gelation process, which encapsulates the phosphor particles dispersed therein.
[0047] In this step, the shape of the product solid luminescent material can be controlled by the treatment method of SiO2 wet gel. If the solid luminescent material is in powder form, then the object of surface modification is a small piece of SiO2 wet gel. With subsequent drying, powdered SiO2 aerogel can be obtained. Specifically, in order to obtain a powdered solid luminescent material, the formed SiO2 wet gel needs to be crushed, and then surface modified, dried, and properly ground to obtain a powdered solid luminescent material. The particle size of the solid luminescent material mainly depends on the size of the phosphor particles and the degree of grinding. If the solid luminescent material is in block form, then the corresponding surface modification is blocky SiO2 wet gel, and blocky SiO2 aerogel can be obtained by drying.
[0048] Optionally, after the surface modification treatment, the pores of the SiO2 wet gel are first filled with a solvent, and then CO2 supercritical drying is performed. The purpose of filling the pores of the SiO2 wet gel with a solvent is to replace the surface modification liquid in the pores and facilitate the subsequent CO2 supercritical drying process.
[0049] It should be noted that both the surface modification and the solvent-filled pores are carried out by slow diffusion of the liquid, and the process is very slow, so there will be no situation where the phosphor particles are washed out.
[0050] The embodiments of the present application also provide an application of the above-mentioned solid luminescent material in white light LEDs, white light LDs, plant lighting lamps or display devices.
[0051] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0052] Example 1
[0053] This embodiment provides a K2SiF6:Mn 4+ -SiO2 aerogel red light composite phosphor, which is prepared according to the following process:
[0054] 0.025 mol of tetraethyl orthosilicate TEOS and 0.175 mol of ethanol were mixed in a polytetrafluoroethylene container, and then 0.025 mol of deionized water and 0.245 mg of oxalic acid were dropped into the container and stirred for 1 hour, and the mixture was allowed to stand at room temperature for 24 hours to form SiO2 sol.
[0055] 1g of red phosphor K2SiF6:Mn 4+ (particle size is about 10 microns) was added to the SiO2 sol and stirred for 5 minutes, followed by adding 0.75 mL of ammonia water and 2.7 mL of deionized water, stirring until viscous and letting stand for 3 hours, then adding 10 mL of ethanol and aging at 50°C for 20 hours to obtain a wet gel.
[0056] The wet gel was crushed and immersed in a mixed solution of 5 mL hexamethyldisilazane and 20 mL n-hexane, stirred at 50 °C for 4 hours to complete the surface modification process; after standing for 3 hours, it was baked in an oven at 100 °C for 3 hours to obtain K2SiF6:Mn 4 + -SiO2 aerogel red light composite phosphor.
[0057] Figure 3 The hydrophobic diagram of the raw phosphor and the coated product phosphor. It can be seen from the figure that K2SiF6:Mn 4+ -SiO2 aerogel red light composite phosphor has a hydrophobic angle of 143°, which is much higher than that of pure red phosphor K2SiF6:Mn 4+ , showing strong hydrophobicity, effectively solving the problem of K2SiF6:Mn 4+ The key issue of failure when exposed to water.
[0058] Figure 4 and Figure 5 K2SiF6:Mn 4+ -XRD diagram and excitation-emission spectrum of SiO2 aerogel red light composite phosphor. Figure 4 The XRD patterns shown include the amorphous SiO2 aerogel and K2SiF6:Mn 4+ The characteristic crystal peaks of Figure 5 The spectrum shown is for the red phosphor K2SiF6:Mn 4+ Characteristic excitation-emission spectrum.
[0059] The K2SiF6:Mn 4+ -SiO2 aerogel red light composite phosphor is packaged with 455nm LED blue light chip to obtain an LED lamp that can be used for plant lighting.
[0060] Example 2
[0061] This embodiment provides a K2SiF6:Mn 4+ -SiO2 aerogel block, which is different from Example 1 in that: in this example, the wet gel is directly surface-modified without being crushed, and then the surface-modified wet gel is washed with n-hexane solvent for multiple times to replace and remove the surface modifier in the pores, and the soaking liquid is prepared in the order of n-hexane and anhydrous ethanol ratios from 1:0, 7:3, 5:5, 3:7, and 0:1 for soaking, so that the anhydrous ethanol gradually fills the pores of the wet gel; then CO2 supercritical drying is performed, and the specific operation is as follows: first, CO2 liquid is used to immerse the block wet gel to replace the anhydrous ethanol in the pores, and after 3 CO2-anhydrous ethanol replacement processes, the pores of the wet gel are completely filled with CO2 liquid; then the block immersed in the CO2 liquid is kept at 1200psi and 35°C for 10 minutes, and then the CO2 gas is slowly discharged to obtain K2SiF6:Mn 4+ -SiO2 aerogel block.
[0062] Figure 6 K2SiF6:Mn 4+ -SiO2 aerogel block under indoor light, 365nm ultraviolet lamp, 405nm laser, 460nm laser irradiation, it can be seen that ultraviolet light and blue light laser can effectively excite the K2SiF6:Mn 4+ -SiO2 aerogel blocks emit bright red light.
[0063] Example 3
[0064] This embodiment provides a K2SiF6:Mn 4+ / β-sialon-SiO2 aerogel red and green light composite phosphor, which is different from Example 1 in that: 0.8g of red phosphor K2SiF6:Mn 4+ At the same time, 1g of green phosphor β-sialon was added, and finally K2SiF6:Mn 4+ / β-sialon-SiO2 aerogel red and green light composite phosphor.
[0065] The K2SiF6:Mn 4+ The red and green composite phosphor of / β-sialon-SiO2 aerogel is packaged with a 455nm LED blue light chip to obtain an LED light source that can be used for display. Its electroluminescence spectrum is as follows Figure 7 As shown; the chromaticity diagram is as Figure 8 As shown, the color coordinates are (0.3162, 0.3332), the color temperature is 6290K, the luminous efficiency is 86.78lm / W, and the color rendering index is 81.8.
[0066] Example 4
[0067] This embodiment provides a K2TiF6:Mn 4+ -SiO2 aerogel red light composite phosphor, which is prepared according to the following process:
[0068] 0.025 mol of tetraethyl orthosilicate TEOS and 0.175 mol of ethanol were mixed in a polytetrafluoroethylene container, and then 0.03 mol of deionized water and 0.25 mg of oxalic acid were dropped into the container and stirred for 1 hour, and the mixture was allowed to stand at room temperature for 24 hours to form SiO2 sol.
[0069] 1g of red phosphor K2TiF6:Mn 4+ Add to SiO2 sol and stir for 5 minutes, then add 0.65mL ammonia water and 3mL deionized water, stir until viscous and let stand for 3 hours, then add 7ml ethanol and age at 50℃ for 20h to obtain wet gel.
[0070] The wet gel was crushed and immersed in a mixed solution of 3 mL hexamethyldisilazane HMDZ and 15 mL n-hexane, stirred at 50 °C for 4 hours to complete the surface modification process; after standing for another 3 hours, it was baked in an oven at 100 °C for 3 hours to obtain K2TiF6:Mn 4+ -SiO2 aerogel red light composite phosphor, its characteristic excitation-emission spectrum is as follows Fig. 9 shown.
[0071] Example 5
[0072] This embodiment provides a K2GeF6:Mn 4+ -SiO2 aerogel red light composite phosphor, which is prepared according to the following process:
[0073] 0.025 mol of tetraethyl orthosilicate TEOS and 0.175 mol of ethanol were mixed in a polytetrafluoroethylene container, and then 0.05 mol of deionized water and 0.3 mg of oxalic acid were dropped into the container and stirred for 1 hour, and the mixture was allowed to stand at room temperature for 24 hours to form a SiO2 sol.
[0074] 1.5g of red phosphor K2GeF6:Mn 4+ Add to SiO2 sol and stir for 5 minutes, then add 0.80mL ammonia water and 5mL deionized water, stir until viscous and let stand for 3 hours, then add 9ml ethanol and age at 50℃ for 20h to obtain wet gel.
[0075] The wet gel was crushed and immersed in a mixed solution of 6 mL hexamethyldisilazane HMDZ and 20 mL n-hexane, stirred at 50 °C for 4 hours to complete the surface modification process; after standing for another 3 hours, it was baked in an oven at 100 °C for 5 hours to obtain K2GeF6:Mn 4+-SiO2 aerogel red light composite phosphor, its characteristic excitation-emission spectrum is as follows Fig.10 shown.
[0076] In summary, the solid luminescent material and its preparation method and application in the embodiment of the present application are A2XF6:Mn 4+ The phosphor particles are evenly dispersed in the pores of the SiO2 aerogel, and the SiO2 aerogel is surface-modified to obtain a super-hydrophobic phosphor-aerogel composite luminescent material. The preparation temperature is low, and the problem of phosphor failure when exposed to water or water vapor can be effectively solved, thereby improving the stability and life of related devices.
[0077] The above description is only an embodiment of the present application and is not intended to limit the protection scope of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A solid luminescent material, characterized in that: The invention comprises SiO2 aerogel and phosphor A2XF6:Mn dispersed in the SiO2 aerogel. 4+ A is selected from one of Na, K, Rb, and Cs, X=one of Si, Ge, Sn, Ti, and Zr, the SiO2 aerogel is a porous structure, and the phosphor A2XF6:Mn 4+ The SiO2 aerogel is dispersed in the pores of the SiO2 aerogel, and the surface of the SiO2 aerogel is also grafted with hydrophobic groups.
2. The solid luminescent material according to claim 1, characterized in that: The particle size of the phosphor is 0.01-30 μm.
3. The solid luminescent material according to claim 1, characterized in that The pore size of the SiO2 aerogel is 1-100 nm, and the porosity is > 99%.
4. The solid luminescent material according to claim 1, characterized in that: The SiO2 aerogel is in the form of powder, block or film.
5. A method for preparing a solid luminescent material as claimed in claim 1, characterized in that: It includes the following steps: SiO2 sol and phosphor A2XF6:Mn 4+ Mix well, and then gel the SiO2 sol to obtain dispersed A2XF6:Mn 4+ SiO2 wet gel; The SiO2 wet gel is subjected to surface modification treatment to graft hydrophobic groups, and then dried to obtain a dispersed fluorescent powder A2XF6:Mn 4+ SiO2 aerogel.
6. The method for preparing a solid luminescent material according to claim 5, characterized in that: The preparation method of SiO2 sol is as follows: dissolving the component raw materials used to form SiO2 aerogel in a solvent, adding a hydrolysis catalyst, stirring, and standing to obtain SiO2 sol.
7. The method for preparing a solid luminescent material according to claim 6, characterized in that: The preparation method of SiO2 aerogel is as follows: disperse the phosphor A2XF6:Mn 4+ Add a polycondensation catalyst to the SiO2 sol and stir evenly. The SiO2 sol gradually solidifies into a gel. Then add an aging liquid to replace the liquid therein and let it stand for aging.
8. The method for preparing a solid luminescent material according to claim 5, characterized in that: The surface modification treatment method is: immersing the SiO2 wet gel in a solution containing a surface modifier.
9. The method for preparing a solid luminescent material according to claim 5, characterized in that: After the surface modification, the pores of the SiO2 wet gel are first filled with a solvent, and then CO2 supercritical drying is performed.
10. Use of the solid luminescent material according to claim 1 in white light LEDs, white light LDs, plant lighting lamps or display devices.