A kind of structural steel with low Ti content and its electroslag remelting method

By applying aluminum powder to the upper part of the electrode base material and using a specific remelting slag system, the problem of large fluctuations in the remelting of electroslag is solved, and low-cost and stable production of low-Ti content is achieved, ensuring the electroslag ingot The uniformity of Ti content and the yield rate are improved.

CN115637332BActive Publication Date: 2024-11-05DAYE SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211350941.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-11-05
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

The existing electroslag remelting technology is difficult to effectively control the content of Ti elements, resulting in large fluctuations in Ti content, especially in the production of low-Ti-content structural steels, resulting in low yield and high cost.

Method used

By applying aluminum powder to the upper part of the electrode base material and using a specific remelting slag system combination, including CaF2, Al2O3, SiO2 and TiO2, the melting point and slag resistance of the slag during the remelting process are controlled to ensure that the Ti content is between 0.04-0.10 % stability.

Benefits of technology

The uniformity and stability of the Ti content of the head, middle and tail of the electroslag ingot is achieved, meeting the requirement of 0.04-0.10%, reducing the burn loss of Ti, improving the yield of the electroslag ingot and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003918837540000061
    Figure BDA0003918837540000061
  • Figure BDA0003918837540000071
    Figure BDA0003918837540000071
  • Figure BDA0003918837540000081
    Figure BDA0003918837540000081
Patent Text Reader

Abstract

The invention provides a low-Ti content structural steel and an electroslag remelting method thereof, comprising the following steps: firstly applying aluminum powder to the middle and upper surface of an electrode base material, and then electroslag remelting the electrode base material to obtain the low-Ti content structural steel; based on the mass of the electrode base material, the Al content in the electrode base material is 0.10-0.12%, and the Ti content is 0.09-0.11%; the remelting slag of the electroslag remelting includes 65%-70% of CaF 2 , 25‑30% Al 2 O 3 , 0.80‑1.5% SiO 2 , 3.5‑5% TiO 2 The present invention controls the content of Ti and Al in the electrode matrix, and stabilizes the Ti melting loss of the matrix during the remelting process. Setting a new remelting slag system solves the problem that the Ti content at the tail of the electroslag ingot is less than 0.04%. Applying aluminum powder on the upper surface of the matrix electrode solves the problem that the Ti content at the head of the electroslag ingot is less than 0.04%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroslag remelting, and in particular relates to a low-Ti content structural steel and an electroslag remelting method thereof. Background Art

[0002] Ti is an easily oxidizable element, and it is difficult to control the Ti element during electroslag remelting. Structural steels containing "0.040-0.10%" Ti are generally single-refined varieties in electric furnaces and converters, and are generally not subjected to electroslag remelting. In recent years, as the market's requirements for metal material cleanliness and uniformity have increased, some Ti-containing structural steels have been produced using electroslag remelting.

[0003] When using the electroslag remelting process, the arc starting end of the electroslag ingot will burn due to the reaction between the Ti in the parent material and the remelting slag, resulting in the Ti content in the steel being less than 0.040%, which is unqualified. As the remelting proceeds, the surface of the parent material continues to oxidize at high temperature, and the oxidation of Ti in the steel increases. In the later stage of remelting, the Ti in the steel burns more and more, making its Ti content less than 0.04%, which is unqualified. Whether it is the electroslag ingot obtained by remelting the same electrode or the electroslag ingot obtained by multiple batches of electrodes, the Ti content at the head and tail of the same electroslag ingot fluctuates greatly, or the Ti content between different electroslag ingots also fluctuates greatly, and the Ti content often cannot meet the "0.040-0.10%" Ti content, resulting in a low electroslag ingot yield.

[0004] In the prior art, when the electroslag remelting method is used to produce structural steel containing more than 0.30% Ti, in order to avoid large burning loss at the arc starting end of the electroslag ingot, it is often necessary to prepare a separate purified slag material (for example, using low carbon steel containing 6-7% Al as the base material, and using fluorite as the slag material for remelting and purification), which is costly. Moreover, when the electroslag remelting is used to prepare structural steel containing more than 0.30% Ti and structural steel with low Ti content (0.04-0.10%), the burning law of Ti is very different. Comprehensively considered, in order to obtain a low-cost method for preparing structural steel containing "0.040-0.10%" Ti by electroslag remelting process, the existing electroslag remelting production process of structural steel containing more than 0.30% Ti has no reference significance.

[0005] Therefore, it is necessary to develop a low-cost electroslag remelting method that is particularly suitable for structural steel containing Ti "0.040-0.10%". Summary of the invention

[0006] In view of the above technical defects, one of the purposes of the present invention is to provide an electroslag remelting method for structural steel with low Ti content, and the second purpose of the present invention is to provide structural steel with low Ti content prepared by the electroslag remelting method. The electroslag remelting method of the present invention can reduce the burning loss of Ti in steel, obtain electroslag ingots with Ti composition that meets the requirements, and the fluctuation range of Ti content in the head, middle and tail of the electroslag ingot is small, and the Ti content can meet the requirement of "0.04-0.1%". In addition, the electroslag remelting method of the present invention is stable and effective.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides an electroslag remelting method for low-Ti content structural steel, comprising the following steps:

[0009] First, aluminum powder is applied to the middle and upper surface of the electrode base material, and then the electrode base material is electroslag remelted to obtain an electroslag ingot; the electroslag ingot is a structural steel with a Ti content of 0.04-0.10wt%;

[0010] Wherein, based on the mass of the electrode base material, the Al content in the electrode base material is 0.10-0.12%, and the Ti content is 0.09-0.11%;

[0011] The electroslag remelting slag system comprises 65%-70% CaF2, 25-30% Al2O3, 0.8-1.5% SiO2, and 3.5-5% TiO2 by mass percentage;

[0012] By controlling the contents of the main components of the slag, CaF2 and Al2O3, in the remelting slag system, the melting point of the slag can be lowered, thus ensuring the "steel-slag" separation during the remelting process.

[0013] The CaF2 in the heavy melting slag system for preparing low-Ti content steel (0.04-0.10%) of the present invention can be prepared with fluorite, and the fluorite does not need to be purified and can be used directly, with low cost.

[0014] SiO2 is a residual component in general slag. The lower the SiO2 content in the slag, the better. If the SiO2 content exceeds 1.5%, it will have a great impact on the burning loss of Ti in the steel.

[0015] TiO2 is an additive. If the TiO2 content is too low, the Ti in the steel will be burned out and the steel will be unqualified. If the TiO2 content is too high, the cost will be increased and the Ti content will increase in serious cases, exceeding the standard and unqualified.

[0016] The remelting slag system used in the present invention does not contain calcium oxide because calcium oxide has strong water absorption and will increase the burning loss of Ti.

[0017] In the above electroslag remelting method, as a preferred embodiment, the mass percentage of the remelting slag system of the electroslag remelting to the mass percentage of the electrode base material is controlled between 4.0-6.0%.

[0018] In the above-mentioned electroslag remelting method, as a preferred implementation mode, the smelting current of the electroslag remelting is 8000-14000A, and the smelting voltage is 32-48V; the specific smelting voltage (furnace mouth voltage) and smelting current settings in each furnace are adaptively adjusted according to the size of the smelting electroslag base material and the size of the electroslag ingot to be obtained.

[0019] For example, the smelting current of electroslag remelting is related to the ingot type (parent material, crystallizer size), 2.5t crystallizer (upper mouth 510*510mm / lower mouth 550*550mm), electrode parent material Ф400mm, remelting current 14000-12500A, maximum remelting current is 14000A (the current decreases within the range of 14000-12500A during the remelting process), and the smelting voltage of electroslag remelting is 42-48V.

[0020] 1.2t crystallizer (upper mouth 410*410mm / lower mouth 450*450mm, four corners arc), electrode base material Ф320mm, melting current 10000-8000A, maximum remelting current is 10000A (the current decreases within the range of 10000-8000A during the remelting process), and the smelting voltage of the electroslag remelting is 32-36V.

[0021] In the above electroslag remelting method, as a preferred embodiment, the slag resistance during the electroslag remelting process is in the range of 3.0-3.5 mΩ, which can ensure that the electrode base material is buried in the slag pool to a depth of about 30-40 mm. By controlling the range of slag resistance, the burnout amount of Ti can be stabilized.

[0022] The slag resistance = smelting voltage (furnace mouth voltage) / smelting current. The specific smelting voltage (furnace mouth voltage) and smelting current in each furnace are adaptively adjusted according to the size of the smelting electroslag parent material and the size of the electroslag ingot to be obtained.

[0023] In the above electroslag remelting method, as a preferred embodiment, the mass of the aluminum powder accounts for 0.02-0.035% of the electrode base material. Aluminum powder is applied to the middle and upper part of the base material to reduce the burning loss of Ti in the later stage of remelting.

[0024] In the above-mentioned electroslag remelting method, as a preferred embodiment, before the electroslag remelting, it also includes a step of slagging using a graphite electrode.

[0025] In the above-mentioned electroslag remelting method, as a preferred embodiment, the slag-melting time is 25-30 minutes.

[0026] In the above electroslag remelting method, the slag melting current and voltage are related to the size of the crystallizer (ingot). As a preferred embodiment, the maximum slag melting current is 5000-6000A, and the maximum voltage is 60-70V;

[0027] For example, 2.5t crystallizer (upper mouth 510*510mm / lower mouth 550*550mm): maximum current 6000A (arc starts at 800A, gradually increases current, reaches maximum current 6000A after 7 minutes to complete slag melting). Maximum voltage (secondary voltage) 70V (arc starts at 52V, gradually increases, reaches maximum voltage 70V after 7 minutes).

[0028] In the above-mentioned electroslag remelting method, as a preferred embodiment, the electrode base material needs to be shot blasted before applying the aluminum powder.

[0029] In the above-mentioned electroslag remelting method, as a preferred embodiment, the preparation method of the electrode base material includes: an electric furnace or converter smelting process, a refining furnace refining process and a die casting process; preferably, an electric furnace smelting and VD refining process.

[0030] In the above electroslag remelting method, as a preferred embodiment, in addition to Al and Ti, other raw materials used to prepare the electrode base material are formulated according to the designed composition of low-Ti content structural steel.

[0031] In a second aspect, the present invention further provides a low-Ti content structural steel prepared by the above-mentioned electroslag remelting method;

[0032] The low Ti content structural steel may be 16Cr2MnTiA, 20Cr1Mo1VNbTiB, 30CrMnMoTiA or the like.

[0033] Compared with the prior art, the present invention has one of the following beneficial effects:

[0034] 1. The present invention provides a low-Ti content structural steel and an electroslag remelting method thereof, comprising the following steps: firstly applying aluminum powder to the middle and upper surface of an electrode base material, and then electroslag remelting the electrode base material to obtain a low-Ti content structural steel; wherein, based on the mass of the electrode base material, the Al content in the electrode base material is 0.10-0.12%, and the Ti content is 0.09-0.11%; the remelting slag system of the electroslag remelting comprises 65%-70% CaF2, 25-30% Al2O3, 0.80-1.5% SiO2, and 3.5-5% TiO2. The present invention controls the content of Ti and Al in the electrode base material, and stabilizes the Ti melting loss of the base material during the remelting process. The present invention reduces the substantial melting loss of Ti in the steel in the early stage of remelting by setting a new remelting slag system, and solves the problem that the Ti content at the tail of the electroslag ingot is less than 0.04%. The present invention reduces the significant melting loss of Ti in the steel in the later stage of remelting by applying aluminum powder on the middle and upper surface of the parent electrode, and solves the problem that the Ti content of the electroslag ingot head is less than 0.04%. The present invention applies aluminum powder on the middle and upper surface of the parent electrode, which can ensure that aluminum is continuously and evenly added during the remelting process of the parent electrode.

[0035] 2. The low-Ti content structural steel and the electroslag remelting method thereof provided by the present invention control the remelting current and remelting voltage during the remelting process to ensure that the slag resistance during the remelting process is 3.0-3.5 mΩ. If the slag resistance value is set too large, the electrode base material is buried shallowly in the slag pool, and the surface temperature of the slag pool is high, thereby aggravating electrode oxidation and affecting the stability of the Ti element recovery rate. If the slag resistance value is set too small, the electrode base material is buried deep in the slag pool, increasing the depth of the metal molten pool under the slag pool, deteriorating the solidification structure of the electroslag ingot, and affecting the surface quality of the electroslag ingot.

[0036] 3. The Ti content in the head, middle and tail of the electroslag ingot obtained by the electroslag remelting method of the present invention all meet the requirement of "0.040-0.10%", and the fluctuation range of the Ti content in the head, middle and tail is small.

[0037] 4. The production control method of electroslag structural steel with low Ti content of the present invention is stable and effective, and the Ti contents of the head, middle and tail of electroslag ingots obtained in multiple batches all meet the requirement of "0.040-0.10%". DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below so that those skilled in the art can practice and reproduce them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art are within the scope of protection of the present invention.

[0039] The electroslag remelting method of the present invention is suitable for preparing any structural steel with a Ti mass content of "0.040-0.10%". For clearer description and comparison, the following embodiments of the present invention are described only by taking the preparation of 30CrMnMoTiA steel as an example.

[0040] The electrode base material used in the following examples is prepared according to the composition content of 30CrMnMoTiA steel, but the specific contents of Ti and Al in the base material and other components shall be subject to the contents recorded in each example. The preparation method of the electrode base material is 20-ton electric furnace smelting + VD refining. The specific smelting and refining methods are conventional processes in the field and will not be repeated here.

[0041] Before electroslag remelting, the upper end of the electrode needs to be fixed on the dummy electrode to facilitate the fixation of the electrode base material and subsequent electroslag remelting. Aluminum powder is coated on one end of the electrode base material close to the dummy electrode (i.e., the upper middle part of the electrode base material).

[0042] All % not otherwise specified in the following examples are by mass percentage.

[0043] Example 1

[0044] Smelting in a 20-ton electric furnace, LF+VD refining, pouring 6 Ø400mm electrode base materials (cast rods), and electroslag remelting of electroslag ingots in a 2.5t crystallizer (upper mouth 510*510mm / lower mouth 550*550mm, four corners arc).

[0045] The smelting composition of the electrode base material is as follows (the balance is Fe and unavoidable impurities):

[0046] element C Mn Si Cr Mo Ti Al Mass% 0.29 0.98 0.27 1.20 0.23 0.10 0.11

[0047] Note: The melting composition of electrode base material refers to the composition of the sample analyzed in the liquid steel before casting the electrode rod after the steel liquid is refined in the electric furnace.

[0048] This embodiment provides an electroslag remelting method for low-Ti content structural steel, comprising the following steps:

[0049] (1) First, select 6 electrode base materials, shot blast them, and then apply aluminum powder on the middle and upper part of the electrode base materials. The diameter of the electrode base materials is 400 mm, the length is 2800 mm, and the mass is 2700 kg. The amount of aluminum powder applied is 600 g / piece (the coating area is about 100 mm wide and about 1200 mm long). The upper edge of the aluminum powder coating area is 20 mm away from the upper end of the electrode base material.

[0050] (2) Graphite electrode slag, maximum slag current 6000A, slag time 30min, maximum slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 6kg titanium dioxide" (126Kg / electrode). In terms of mass percentage, CaF2 accounts for 65.66%, Al2O3 accounts for 28.29%, SiO2 accounts for 1.34%, and TiO2 accounts for 4.71%.

[0051] (3) After slag melting, the six electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum current of electroslag remelting is 14000A, and the furnace mouth voltage is 42-48V (this value is a range value, the voltage is high in the early stage of remelting and low in the later stage); the size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0052] Based on the mass of the electroslag ingot, the Ti and Al contents at the head and tail of the six electroslag ingots tested were within the range of 0.0471-0.0668%. The specific test results are as follows:

[0053]

[0054] Note: The other elements [C], [Mn], [Si], [Cr], and [Mo] all meet the standard requirements of 30CrMnMoTiA steel, and there is no increase in silicon content.

[0055] Example 2

[0056] Smelting in a 20-ton electric furnace, LF+VD refining, pouring 13 φ320mm electrode base materials (cast rods), and electroslag remelting of electroslag ingots in a 1.2t crystallizer (upper mouth 410*410mm / lower mouth 450*450mm, four corners arc).

[0057] The smelting composition of electrode base material is as follows:

[0058] element C Mn Si Cr Mo Ti Al Mass% 0.32 1.05 0.33 1.18 0.24 0.094 0.10

[0059] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0060] This embodiment provides an electroslag remelting method for low-Ti content structural steel, comprising the following steps:

[0061] (1) 13 electrode base materials were selected, and after shot blasting, aluminum powder was applied to the middle and upper parts of the electrode base materials. The diameter of the electrode base materials was 320 mm, the length was 2100 mm, and the mass was 1320 kg. The amount of aluminum powder applied was 400 g / piece (the coating area was about 80 mm wide and about 1200 mm long). The upper edge of the aluminum powder coating area was 20 mm away from the upper end of the electrode base material.

[0062] (2) Graphite electrode slag, maximum slag current 5000A, slag time 25min, maximum slag voltage 60V. The remelting slag material is "49kg fluorite + 21Kg alumina powder + 3kg titanium dioxide" (73Kg / piece), and the remelting slag system contains 66.45% CaF2, 28.48% Al2O3, 1.0% SiO2, and 4.07% TiO2.

[0063] (3) After slag melting, 13 electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum electroslag remelting current is 10000A, and the furnace mouth voltage is 32-36V. The size of the crystallizer is 410*410mm at the upper mouth and 450*450mm at the lower mouth.

[0064] Based on the mass of the electroslag ingot, the Ti and Al contents at the head and tail of 13 electroslag ingots were tested. The fluctuation range of Ti content was 0.0434-0.0611%. The specific test results are as follows:

[0065]

[0066]

[0067] Note: The other elements [C], [Mn], [Si], [Cr], and [Mo] all meet the standard requirements of 30CrMnMoTiA steel, and there is no increase in silicon content.

[0068] Example 3

[0069] Smelting in a 20-ton electric furnace, LF+VD refining, pouring 6 Ø400mm electrode base materials (cast rods), and electroslag remelting of electroslag ingots in a 2.5t crystallizer (upper mouth 510*510mm / lower mouth 550*550mm, four corners arc).

[0070] The smelting composition of electrode base material is as follows:

[0071] element C Mn Si Cr Mo Ti Al Mass% 0.30 1.02 0.30 1.22 0.24 0.10 0.12

[0072] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0073] This embodiment provides an electroslag remelting method for low-Ti content structural steel, comprising the following steps:

[0074] (1) Six electrode matrix materials were selected, and after shot blasting, aluminum powder was applied to the middle and upper parts of the electrode matrix materials. The diameter of the electrode matrix materials was 400 mm, the length was 2800 mm, and the mass was 2700 kg. The amount of aluminum powder applied was 700 g / piece (the coating area was about 100 mm wide and about 1200 mm long). The upper edge of the aluminum powder coating area was 20 mm away from the upper end of the electrode matrix materials.

[0075] (2) Graphite electrode slag, maximum slag current 6000A, slag time 30min, maximum slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 6kg titanium dioxide" (126Kg / electrode). In terms of mass percentage, CaF2 accounts for 65.66%, Al2O3 accounts for 28.29%, SiO2 accounts for 1.34%, and TiO2 accounts for 4.71%.

[0076] (3) After slag melting, the six electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum current of electroslag remelting is 14000A, and the furnace mouth voltage is 42-48V (this value is a range value, the voltage is high in the early stage of remelting and low in the later stage); the size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0077] Based on the mass of the electroslag ingot, the Ti and Al contents at the head and tail of the six electroslag ingots tested were within the range of 0.0646-0.0898%. The specific test results are as follows:

[0078]

[0079] Note: The other elements [C], [Mn], [Si], [Cr], and [Mo] all meet the standard requirements of 30CrMnMoTiA steel, and there is no increase in silicon content.

[0080] Comparative Example 1

[0081] The Ti content of the electrode base material was increased to 0.14%, and the electroslag remelting method of low-Ti content structural steel was used to compare the Ti content on the electroslag ingot.

[0082] The melting composition of electrode base material (Ø400mm) is as follows

[0083] element C Mn Si Cr Mo Ti Al Mass% 0.31 1.00 0.31 1.20 0.23 0.14 0.115

[0084] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0085] The electroslag remelting method of the low Ti content structural steel in this comparative example comprises the following steps:

[0086] (1) Three electrode matrix materials were selected and, after shot blasting, aluminum powder was applied to the middle and upper parts of the electrode matrix materials. The diameter of the electrode matrix materials was 400 mm, the length was 2800 mm, and the mass was 2700 kg. The amount of aluminum powder applied was 600 g / piece (the coating area was about 100 mm wide and about 1200 mm long). The upper edge of the aluminum powder coating area was 20 mm away from the upper end of the electrode matrix materials.

[0087] (2) Graphite electrode slag, maximum slag current 6000A, slag time 30min, maximum slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 6kg titanium dioxide" (126Kg / electrode). In terms of mass percentage, CaF2 accounts for 65.66%, Al2O3 accounts for 28.29%, SiO2 accounts for 1.34%, and TiO2 accounts for 4.71%.

[0088] (3) After slag melting, the three electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum current of electroslag remelting is 14000A, and the furnace mouth voltage is 42-48V; the size of the crystallizer is 510*510mm at the upper mouth and 550*550mm at the lower mouth.

[0089] Based on the mass of the electroslag ingot, the contents of Si, Ti and Al at the head and tail of the three electroslag ingots tested, the fluctuation range of Ti content is 0.0846-0.1215%, and the specific test results are as follows:

[0090]

[0091] The Si content at the tail of the electroslag ingot is 0.04-0.05% higher than that of the electrode base material, and the Ti content is less than 0.1%; while the Ti content at the head of the electroslag ingot has exceeded 0.1%, which is unqualified.

[0092] The inventors have also proved through other experiments that if the Ti of the electrode base material is further increased (Ti≥0.15%) and the low-cost slag of the present invention is used for remelting, the tail of the electroslag ingot will increase [Si] more, and the Si content will exceed 0.37% (the standard requires Si: 0.17-0.37%), which is unqualified.

[0093] Comparative Example 2

[0094] If the Al content of the electrode base material is too low or too high, the composition of the remelted electroslag ingot will be affected.

[0095] The melting composition of electrode base material (Ø400mm) is as follows

[0096] Elemental composition C Mn Si Cr Mo Ti Al Electrode base material 1 0.30 1.03 0.32 1.18 0.23 0.10 0.05 Electrode base material 2 0.32 1.04 0.31 1.15 0.24 0.10 0.15

[0097] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0098] The electroslag remelting method of the low Ti content structural steel in this comparative example comprises the following steps:

[0099] (1) Select three electrode base materials 1 and 2 respectively, and after shot blasting the electrode base materials, apply aluminum powder on the middle and upper part of the electrode base materials. The diameter of the electrode base material is 400 mm, the length is 2800 mm, and the mass is 2700 kg. Based on the mass of the electrode base material 1, the Ti content in the electrode base material is 0.10%, the Al content is 0.05%, and the application amount of aluminum powder is 800 g / piece (the coating area is about 100 mm wide and about 1200 mm long), and the upper edge of the aluminum powder coating area is 20 mm away from the upper end of the electrode base material.

[0100] The Ti content in the electrode base material 2 is 0.10%, the Al content is 0.15%, the application amount of aluminum powder is 200g / stick (the coating area is about 100mm wide and about 500mm long), and the upper edge of the aluminum powder coating area is 20mm away from the upper end of the electrode base material.

[0101] (2) Graphite electrode slag, maximum slag current 6000A, slag time 30min, maximum slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 6kg titanium dioxide" (126Kg / electrode). In terms of mass percentage, CaF2 accounts for 65.66%, Al2O3 accounts for 28.29%, SiO2 accounts for 1.34%, and TiO2 accounts for 4.71%.

[0102] (3) After slag melting, the three electrode base materials 1 and 2 are electroslag remelted to obtain electroslag ingots. The maximum current of electroslag remelting is 14000A, and the furnace mouth voltage is 42-48V. The size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0103] Based on the mass of the electroslag ingot, the contents of Si, Ti and Al at the head and tail of the six electroslag ingots were tested. The test results are as follows:

[0104]

[0105]

[0106] The Ti content of the tail of the electroslag ingot remelted from low-Al electrode base metal is less than 0.04%, which is unqualified. The Ti content of the electroslag ingot remelted from high-Al electrode base metal is qualified, but the tail of the electroslag ingot increases [Si], and the Si content exceeds 0.37% (the standard requires Si: 0.17-0.37%), which is unqualified.

[0107] Comparative Example 3

[0108] If the upper part of the electrode base material is not coated with aluminum powder, the composition of the remelted steel ingot.

[0109] The melting composition of electrode base material (Ø400mm) is as follows

[0110] Elemental composition C Mn Si Cr Mo Ti Al Electrode base material 0.32 1.01 0.32 1.20 0.23 0.10 0.11

[0111] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0112] The electroslag remelting method of the low Ti content structural steel in this comparative example comprises the following steps:

[0113] (1) Three electrode base materials were selected and shot blasted. The electrode base materials had a diameter of 400 mm, a length of 2800 mm, and a mass of 2700 kg. Based on the mass of the electrode base materials, the Ti content in the electrode base materials was 0.10%, the Al content was 0.11%, and no aluminum powder was applied.

[0114] (2) Graphite electrode slag, maximum slag current 6000A, slag time 30min, maximum slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 6kg titanium dioxide" (126Kg / electrode). In terms of mass percentage, CaF2 accounts for 65.66%, Al2O3 accounts for 28.29%, SiO2 accounts for 1.34%, and TiO2 accounts for 4.71%.

[0115] (3) After slag melting, the three electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum electroslag remelting current is 14000A, and the furnace mouth voltage is 42-48V. The size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0116] Based on the mass of the electroslag ingot, the Ti and Al contents at the head and tail of the three electroslag ingots were tested. The test results are as follows:

[0117]

[0118] The Ti content of the head of the remelted electroslag ingot without coating aluminum powder on the upper part of the electrode base material is all less than 0.04%, which is unqualified.

[0119] Comparative Example 4

[0120] Al is directly added to the slag system without increasing the Al content in the electrode base material.

[0121] The melting composition of electrode base material (Ø400mm) is as follows

[0122] Elemental composition C Mn Si Cr Mo Ti Al Electrode base material 0.30 1.00 0.32 1.20 0.23 0.10 0.02

[0123] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0124] The electroslag remelting method of the low Ti content structural steel in this comparative example comprises the following steps:

[0125] (1) Three electrode base materials were selected and shot blasted. The electrode base materials had a diameter of 400 mm, a length of 2800 mm, and a mass of 2700 kg. Based on the mass of the electrode base materials, the Ti content in the electrode base materials was 0.10% and the Al content was 0.02%.

[0126] (2) Graphite electrode slag, slag current 6000A, slag time 30min, slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 6kg titanium dioxide + 4Kg aluminum powder" (130Kg / electrode). According to mass percentage, CaF2 accounts for 63.64%, Al2O3 accounts for 27.42%, SiO2 accounts for 1.30%, TiO2 accounts for 4.56%, and Al accounts for 3.08%. Aluminum powder is added to the slag, and after melting, most of it is oxidized, and part of it reduces SiO2, Si enters the steel, and very little Al remains.

[0127] (3) After slag melting, the three electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum electroslag remelting current is 14000A, and the furnace mouth voltage is 42-48V. The size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0128] Based on the mass of the electroslag ingot, the contents of Si, Ti and Al at the head and tail of the three electroslag ingots were tested. The test results are as follows:

[0129]

[0130] The Ti content in the head and tail of the electroslag ingot is all lower than 0.04%, and the Si content in the tail is all higher than 0.37%, which is unqualified.

[0131] Comparative Example 5

[0132] This comparative example uses slag with a lower TiO2 content for remelting.

[0133] The melting composition of electrode base material (Ф400mm) is as follows:

[0134] Elemental composition C Mn Si Cr Mo Ti Al Electrode base material 0.30 1.00 0.32 1.19 0.22 0.10 0.11

[0135] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0136] (1) Three electrode base materials were selected and shot blasted. The electrode base materials had a diameter of 400 mm, a length of 2800 mm, and a mass of 2700 kg. Based on the mass of the electrode base materials, the Ti content in the electrode base materials was 0.10% and the Al content was 0.11%.

[0137] (2) Graphite electrode slag, slag current 6000A, slag time 30min, slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 3kg titanium dioxide" (123Kg / electrode). In terms of mass percentage, CaF2 accounts for 67.29%, Al2O3 accounts for 28.93%, SiO2 accounts for 1.37%, and TiO2 accounts for 2.41%.

[0138] (3) After slag melting, the three electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum electroslag remelting current is 14000A, and the furnace mouth voltage is 42-48V. The size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0139] Based on the mass of the electroslag ingot, the Ti and Al contents at the head and tail of the three electroslag ingots were tested. The test results are as follows:

[0140]

[0141]

[0142] When the electroslag ingot was remelted using slag with a low TiO2 content of 2.41%, the Ti content at the tail was all less than 0.04%, which was unqualified.

[0143] Comparative Example 6

[0144] This comparative example uses slag with a higher TiO2 content for remelting.

[0145] The melting composition of electrode base material (Ø400mm) is as follows

[0146] Elemental composition C Mn Si Cr Mo Ti Al Electrode base material 0.30 1.00 0.32 1.19 0.22 0.10 0.11

[0147] Note: The melting composition of electrode base material refers to the composition of samples taken from the liquid steel for analysis before casting electrode rods after the steel liquid is refined in the electric furnace.

[0148] (1) Three electrode base materials were selected and shot blasted. The electrode base materials had a diameter of 400 mm, a length of 2800 mm, and a mass of 2700 kg. Based on the mass of the electrode base materials, the Ti content in the electrode base materials was 0.10% and the Al content was 0.11%.

[0149] (2) Graphite electrode slag, slag current 6000A, slag time 30min, slag voltage 70V. The remelting slag material of each electrode is "84kg fluorite + 36Kg alumina powder + 10kg titanium dioxide" (130Kg / electrode). In terms of mass percentage, CaF2 accounts for 63.61%, Al2O3 accounts for 27.35%, SiO2 accounts for 1.36%, and TiO2 accounts for 7.68%.

[0150] (3) After slag melting, the three electrode base materials are electroslag remelted to obtain electroslag ingots. The maximum electroslag remelting current is 14000A, and the furnace mouth voltage is 42-48V. The size of the crystallizer is 510*510mm for the upper mouth and 550*550mm for the lower mouth.

[0151] Based on the mass of the electroslag ingot, the Ti and Al contents at the head and tail of the three electroslag ingots were tested. The test results are as follows:

[0152]

[0153]

[0154] When using slag with a high TiO2 content of 7.68% to remelt the electroslag ingot, the Ti content at the tail is all higher than 0.10%, which is unqualified.

[0155] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.

Claims

1. An electroslag remelting method for low Ti content structural steel, It is characterized in that The following steps are included: First, aluminum powder is applied to the middle and upper surface of the electrode base material, and then the electrode base material is electroslag remelted to obtain an electroslag ingot; the electroslag ingot is a structural steel with a Ti content of 0.04-0.10wt%; Wherein, based on the mass of the electrode base material, the Al content in the electrode base material is 0.10-0.12%, and the Ti content is 0.09-0.11%; The electroslag remelting slag system comprises 65%-70% CaF 2 , 25-30% Al 2 O 3 , 0.8-1.5% SiO 2 , 3.5-5% TiO 2 ; During the electroslag remelting process, the slag resistance is in the range of 3.0-3.5 mΩ; Calculated based on the mass of the electrode base material, the mass of the aluminum powder accounts for 0.02-0.035% of the electrode base material.

2. The electroslag remelting method of low Ti content structural steel according to claim 1, It is characterized in that The mass percentage of the remelting slag system of the electroslag remelting to the mass percentage of the electrode base material is controlled between 4.0-6.0%.

3. The electroslag remelting method of low Ti content structural steel according to claim 1, It is characterized in that The smelting current of the electroslag remelting is 8000-14000A, and the smelting voltage is 32-48V.

4. The electroslag remelting method of low Ti content structural steel according to claim 1, It is characterized in that Before the electroslag remelting, the method further includes a step of using a graphite electrode to perform slag removal.

5. The electroslag remelting method of low Ti content structural steel according to claim 4, It is characterized in that The slag-forming time is 25-30min; The maximum current of the slag-melting is 5000-6000A, and the maximum voltage is 60-70V.

6. The electroslag remelting method of low Ti content structural steel according to claim 1, It is characterized in that Before applying aluminum powder, the electrode base material needs to be shot blasted.

7. The electroslag remelting method of low Ti content structural steel according to claim 1, It is characterized in that The preparation method of the electrode base material comprises: an electric furnace or converter smelting process, a refining furnace refining process and a die casting process.

8. The electroslag remelting method of low Ti content structural steel according to claim 1, It is characterized in that Except Al and Ti, other raw materials used to prepare the electrode base material are formulated according to the designed composition of structural steel with low Ti content.

9. A structural steel with low Ti content prepared by the electroslag remelting method according to any one of claims 1 to 8.