Composite coating facilitating collection and recognition of laser radar sensor and preparation method and application of composite coating

By spraying easy-to-identify functional compositions on metal primer, the angular sensitivity of the high-gloss metal surface is reduced, the reflection intensity and stability of the lidar signal are improved, and the signal drop problem of lidar in metal surface detection is solved. Enhanced recognition capabilities for scenarios such as autonomous driving.

CN119039838AActive Publication Date: 2024-11-29NIPPON PAINT CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410180259.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-18
Publication Date
2024-11-29
Estimated Expiration
2044-02-18

AI Technical Summary

Technical Problem

High-gloss metal surfaces or coatings with metal texture are strong in lidar detection, resulting in a decrease in signal reflection intensity and quantity, affecting the data reliability and safety of lidar.

Method used

Using a composite coating, including metal primer and spray-coated, the composition contains acrylic resin, amino resin, silane coupling agent, high refractive index microbeads and additives, by Spray the easy-to-identify layer to reduce angle sensitivity and improve the reflection intensity of the lidar signal.

Benefits of technology

It significantly improves the reflection intensity and stability of the lidar signal, enhances the signal acquisition capability at different incident angles, improves the identification redundancy and safety guarantee of scenarios such as autonomous driving, and also has excellent mechanical properties, durability and corrosion resistance. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004703560660000061
    Figure BDA0004703560660000061
  • Figure BDA0004703560660000071
    Figure BDA0004703560660000071
  • Figure BDA0004703560660000072
    Figure BDA0004703560660000072
Patent Text Reader

Abstract

The invention discloses a composite coating facilitating collection and recognition of a laser radar sensor and a preparation method and application of the composite coating. The composite coating comprises a bottom coating and a transparent or semitransparent easily-recognized layer sprayed on the bottom coating. The bottom coating is obtained by spraying metal primer; the easy-to-recognize layer is obtained by spraying an easy-to-recognize functional composition, and the easy-to-recognize functional composition comprises the following raw materials in parts by weight: 15-60 parts of acrylic resin; 5-20 parts of amino resin; 0-5 parts of a silane coupling agent; 15 to 45 parts of microbeads with high refractive index; 1-10 parts of an auxiliary agent; and 2-20 parts of a solvent. The composite coating provided by the invention can be directly sprayed on the surface of a metal base material or a non-metal base material, so that the angle sensitivity of the metal base material or a metal primer to a laser radar signal can be reduced, the stability of the reflection intensity of the composite coating to the laser radar signal is ensured, and the reflection intensity of the composite coating to the laser radar signal can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and more specifically, to a composite coating that is beneficial to the acquisition and identification of a laser radar sensor, and a preparation method and application thereof. Background Art

[0002] The development of modern science and technology has gone through the process of mechanization, electrification, informatization and today's intelligentization. Among them, intelligent robots have been applied to various fields in recent years, and advanced robots with higher intelligent perception capabilities and the ability to perform complex tasks have also become a research and development hotspot. It is conceivable that in the future, highly intelligent robots may be seen in various fields, such as infrastructure construction and maintenance, high-end manufacturing, and even the service industry. For example, the self-driving cars that have developed rapidly in recent years are also a form of intelligent robots in a broad sense, that is, smart cars. Smart cars use advanced perception technology and computer analysis systems, decision systems and control systems to effectively cooperate to automatically complete actions such as cruising, merging, avoiding or overtaking.

[0003] Because the robot is a feedback closed-loop control system, if we ignore its scenario-based application design, its core technologies and components can be summarized into four parts: the main structure, the perception device system, the decision-making and planning scheduling system, and the control execution system. The so-called perception device system can be considered as the "eyes" of the robot. These "eyes" can help the robot perceive environmental information and make corresponding decisions. For example, a sweeping robot needs to move from point A to point B and complete the cleaning task. In route planning, it needs to understand where there are obstacles around in order to know how to avoid them. For example, the robot in the hotel lobby needs to identify some indicative signs on the ground to find the route to follow.

[0004] LiDAR technology is a sensor technology with the characteristics of long-range recognition, high resolution, and no influence from ambient light. It is currently widely used in smart cars equipped with higher-level autonomous driving or assisted driving systems. As one of the main sensing devices, it helps smart cars to identify the environment through fusion perception solutions. This route has become the mainstream approach and has been adopted by many OEMs. Similar smart robots, such as delivery robots in hospitals and hotels, or smart sweeping robots for home use, are also equipped with corresponding models of LiDAR sensors to scan and draw route maps and identify obstacles.

[0005] The scanning principle of LiDAR is to obtain raw data by emitting laser of a specific wavelength through a laser and receiving the reflected signal from the surface of an object through a receiver. The mainstream time-of-flight (TOF) mode measures the distance between an object and the signal source based on the time required for the return signal. Through multi-line high-frequency scanning LiDAR, a high-resolution data point cloud in three-dimensional space can be obtained.

[0006] Although LiDAR equipment uses different technical routes, under the same equipment and environmental conditions, the signal strength received by the LiDAR is directly related to the reflectivity of the measured environmental objects to the light source laser. In other words, the reflective characteristics of the object surface will directly affect the detection distance and accuracy of the LiDAR, that is, the detectability will be very different, which will in turn affect the entire perception process.

[0007] Materials or coatings with metallic surface effects and textures are widely used in various decorative coating fields due to their unique appearance, such as automobile bodies, electronic device housings, and household appliance bodies. This metal or simulated metal appearance and texture has long been loved by consumers and has great market value. Metal plating, electroplating or spraying of metallic paint is a common method for preparing surface coatings with metallic appearance and texture, wherein metallic paint is mainly obtained by adding flaky aluminum powder, copper powder pigments or other similar metallic effect pigments such as pearlescent mica to the coating formula. This type of metal sequins, due to its high-gloss surface, will produce a strong specular reflection effect on the incident light signal, just like the metal substrate. For the incident signal of non-visible light source such as laser radar signal, metallic paint and metal substrate will also produce a strong specular reflection effect, which can make the vertical incident laser radar signal almost completely reflected. Therefore, the high-gloss metal substrate or the coating with metallic surface effects and texture is very easy to be detected by the laser radar within a certain distance range and perpendicular to the incident direction of the laser radar sensor.

[0008] However, for various driving scenarios such as autonomous driving, there are not many opportunities for LiDAR signals to be incident on the surface of an object in a vertical direction. First of all, the shapes of cars and other vehicles are irregular and not on the same plane. Most of the surfaces of objects detected by LiDAR are also irregular and not on the same plane. Secondly, as the detection distance increases, the spacing between the beams emitted by the LiDAR increases, the number of effective beams gradually decreases, and the edge part will not be received by the receiver due to the mirror reflection effect. Therefore, for high-gloss metal surfaces or coated surfaces with metallic texture and appearance, for detector signals incident at a certain angle to the plane normal, as the angle increases, the strength and number of returned signals will drop significantly. This is the strong angle sensitivity, which makes it extremely unfavorable for effective detection in various driving scenarios. For LiDAR, the received data pixels will become more volatile due to changes in angles, and the effectiveness will decrease until the data reliability is difficult to predict, which is not conducive to the judgment and decision-making of the decision-making system, and it is very easy to cause detection failure, thereby affecting safety.

[0009] In view of this, there is a need to provide an easily identifiable coating that has good stability under detection at different angles and can be directly used to improve the surface of the coating with a metallic appearance and texture, so that it still has a high and stable reflection intensity for the laser radar detection signal with gradually increasing incident angles. Summary of the invention

[0010] To solve the above problems, the first purpose of the present invention is to provide a composite coating that is conducive to the collection and identification of laser radar sensors. Spraying the composite coating provided by the present invention directly on the substrate can significantly improve the reflection intensity of the composite coating to the laser radar signal, and can also reduce the adverse effects of the strong angle sensitivity of the metal substrate and the metal primer in the composite coating, thereby providing higher recognition redundancy and safety protection for various driving scenarios such as autonomous driving.

[0011] The second object of the present invention is to provide a method for preparing the composite coating as described above.

[0012] The third object of the present invention is to provide an application of the composite coating.

[0013] In order to achieve the above first object, the present invention adopts the following technical scheme:

[0014] The present invention discloses a composite coating that is beneficial to the collection and identification of a laser radar sensor, comprising a base coating and a transparent or translucent easy-to-identify layer sprayed thereon;

[0015] The base coating is obtained by spraying a metal primer;

[0016] The easy-to-identify layer is obtained by spraying an easy-to-identify functional composition, and the easy-to-identify functional composition includes the following raw materials in parts by weight:

[0017] 15-60 parts of acrylic resin;

[0018] 5-20 parts of amino resin;

[0019] Silane coupling agent 0-5 parts;

[0020] 15-45 parts of high refractive index micro beads;

[0021] 1 to 10 parts of additives;

[0022] 2 to 20 parts of solvent.

[0023] Furthermore, the high refractive index microbeads account for 15 to 45 wt % of the total weight of the easy-to-identify functional composition.

[0024] Furthermore, the refractive index of the high-refractive-index microbeads in the near-infrared spectral region is not less than 1.75.

[0025] Furthermore, the refractive index of the high-refractive-index microbeads in the near-infrared spectral region is not less than 1.9.

[0026] Furthermore, the refractive index of the high refractive index microbeads in the near infrared spectrum region is between 1.9 and 2.7.

[0027] Furthermore, the particle size of the high refractive index microbeads is 0.01 to 350 μm.

[0028] Furthermore, the particle size of the high refractive index microbeads is 0.1 to 50 μm.

[0029] Furthermore, the high refractive index microspheres are selected from one or a combination of high refractive index glass microspheres, high refractive index optically transparent ceramic microspheres, and high refractive index amorphous polymer microspheres.

[0030] Furthermore, the high refractive index microspheres are selected from CX-1000 high refractive index glass microspheres produced by Weicaixiang Technology Co., Ltd.

[0031] Further, the acrylic resin is selected from EMA-1032 and / or EMA-1015 of Nippon Paint Co., Ltd.; the amino resin is selected from CYMEL250 and / or CYMEL370N of Cytec Chemicals;

[0032] The silane coupling agent is selected from one or a combination of KH-550, KH-560, KH-570, KH-580, KH-590, KH-902, KH-792 and KH-903 of Dow Corning;

[0033] The auxiliary agent includes one or a combination of antioxidants, light aging agents and leveling dispersants.

[0034] Furthermore, the antioxidant is selected from BASF's B215; the light aging agent is selected from Lianlong's UV944; the leveling dispersant is selected from BYK-345, BYK-187, BYK-192 or a combination of several thereof.

[0035] Furthermore, the metal primer is selected from AR3500(T) silver primer produced by Nippon Paint.

[0036] In order to achieve the above second purpose, the present invention adopts the following technical solutions:

[0037] The present invention discloses a method for preparing the composite coating as described above, comprising the following steps:

[0038] Spray metal primer on the surface of the substrate to obtain a base coat after the surface is dried;

[0039] Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried;

[0040] The coating is dried naturally or baked at room temperature to completely dry the base coating and the easy-to-identify layer to obtain a composite coating.

[0041] Further, the substrate is selected from a metal substrate or a non-metal substrate;

[0042] The metal substrate is selected from tinplate or stainless steel; the non-metal substrate is selected from PP plastic plate.

[0043] In order to achieve the third object, the present invention adopts the following technical solutions:

[0044] The present invention discloses an application of the composite coating as described above in the painting of intelligent vehicles and intelligent robots.

[0045] The beneficial effects of the present invention are as follows:

[0046] The present invention provides a composite coating that is beneficial to the collection and identification of a laser radar sensor. By spraying an easily identifiable functional composition containing high-refractive index microbeads on a metal primer, not only the reflection intensity of the laser radar signal is improved, but also the adverse effects of the strong angle sensitivity of the metal substrate and the metal primer in the composite coating are reduced, so that the reflectivity signal stability of the laser signal at different incident angles is significantly enhanced, and the fluctuation range of the reflectivity signal is reduced. Accordingly, the laser radar sensor can more easily collect more data pixel points returned on the surface involved, thereby obtaining richer obstacle information, so as to ensure that autonomous driving or smart devices can recognize identification and successfully avoid obstacles.

[0047] The composite coating provided by the present invention also has excellent mechanical properties, durability, aging resistance and corrosion resistance, and the composite coating provided by the present invention is transparent or translucent, has little effect on the appearance of the metal, and has a good appearance. Therefore, in many scenarios matching smart cars or smart robot systems, it can be used as a surface coating for various facilities, and can provide decoration and protection at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] The specific implementation modes of the present invention will be further described in detail below in conjunction with the accompanying drawings.

[0049] Figure 1 A schematic diagram showing the structures of different test samples in the laser radar reflectivity test of the present invention.

[0050] Figure 2 A schematic diagram showing the fixing of a test sample on a sample test stand in the laser radar reflectivity test of the present invention.

[0051] Figure 3A schematic diagram showing a method for testing the reflection intensity of a laser radar signal in a laser radar reflectivity test of the present invention. DETAILED DESCRIPTION

[0052] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0053] Unless otherwise specified, parts and parts refer to parts by weight. The experimental materials and reagents used in the following examples can be obtained from commercial channels unless otherwise specified.

[0054] In the present invention, angle sensitivity refers to the degree of fluctuation of the reflection intensity presented by the substrate or coating to the laser radar signal at different incident angles. When the fluctuation of the reflection intensity presented by the laser radar signal at different incident angles is large, the substrate and coating are considered to have strong angle sensitivity to the laser radar signal. Otherwise, the substrate and coating are considered to have weak angle sensitivity to the laser radar signal. Due to the mirror reflection effect of the metal substrate and the coating with a metallic texture and appearance, they will show strong angle sensitivity, which will seriously hinder the collection and recognition of the laser radar sensor in actual application scenarios.

[0055] In order to solve the angle sensitivity problem of metal substrates and coatings with metal texture and appearance, the present invention provides a composite coating that is conducive to the acquisition and recognition of a laser radar sensor, the composite coating comprising a base coating and a transparent or translucent easy-to-identify layer sprayed thereon;

[0056] The base coating is obtained by spraying a metal primer;

[0057] The easy-to-identify layer is obtained by spraying an easy-to-identify functional composition, and the easy-to-identify functional composition includes the following raw materials in parts by weight:

[0058] 15-60 parts of acrylic resin;

[0059] 5-20 parts of amino resin;

[0060] Silane coupling agent 0-5 parts;

[0061] 15-45 parts of high refractive index micro beads;

[0062] 1 to 10 parts of additives;

[0063] 2 to 20 parts of solvent.

[0064] The study found that the composite coating of the present invention, under the joint action of the high refractive index microbeads in the metal primer and the easy-to-identify functional composition, improves the reflection intensity of the composite coating to the laser radar signal, especially for non-metallic substrates such as PP plastics, more effective return signals can be obtained. In addition, in order to reduce the adverse effects of the strong angle sensitivity of the metal substrate and the metal primer in the composite coating, and ensure the stability of the reflectivity signal of the laser signal at different incident angles, the technicians unexpectedly found that the above problems can be solved by spraying the easy-to-identify functional composition directly on the metal primer. Compared with the multi-layer design method used in the prior art, that is, coating the middle coating, topcoat layer, etc. on the metal substrate or metal primer, and covering the problem of the strong angle sensitivity of the metal substrate or metal primer as much as possible, the composite coating of the present invention can save the development cost, time cost and raw material cost of the intermediate layers such as the middle coating and topcoat layer, shorten the process route of the coating spraying, and no longer need to consider the interlayer adhesion, interlayer matching and covering property caused by the intermediate layers such as the middle coating and topcoat layer. A series of problems provide a new direction for the development of coatings that can be identified by laser radar sensors.

[0065] Furthermore, the high refractive index microbeads account for 15 to 45 wt % of the total weight of the easy-to-identify functional composition.

[0066] Furthermore, the refractive index of the high refractive index microbeads provided by the present invention in the near-infrared spectral region (800-2500nm) is not less than 1.75. Preferably, the refractive index of the high refractive index microbeads provided by the present invention in the near-infrared spectral region is not less than 1.9. More preferably, the refractive index of the high refractive index microbeads provided by the present invention in the near-infrared spectral region is between 1.9 and 2.7.

[0067] Furthermore, the particle size of the high refractive index microbeads provided by the present invention is 0.01 to 350 μm, and preferably, the particle size of the high refractive index microbeads provided by the present invention is 0.1 to 50 μm.

[0068] Furthermore, the high refractive index microspheres are selected from one or a combination of high refractive index glass microspheres, high refractive index optically transparent ceramic microspheres, and high refractive index amorphous polymer microspheres.

[0069] In a specific embodiment, the high refractive index microspheres are selected from CX-1000 high refractive index glass microspheres produced by Weicaixiang Technology Co., Ltd. The high refractive index optically transparent ceramic microspheres and high refractive index amorphous polymer microspheres can be prepared by methods disclosed in the prior art.

[0070] Further, the easy identification functional composition comprises 40-50 parts of acrylic resin; the acrylic resin is selected from EMA-1032 and / or EMA-1015 of Nippon Paint Co., Ltd. In a specific embodiment, the easy identification functional composition comprises 10-35 parts of EMA-1032 and 5-25 parts of EMA-1015, preferably, the easy identification functional composition comprises 20-35 parts of EMA-1032 and 10-25 parts of EMA-1015.

[0071] Further, the easy identification functional composition comprises 10-20 parts of amino resin; the amino resin is selected from CYMEL250 and / or CYMEL370N of Cytec Chemical. In a specific embodiment, the easy identification functional composition comprises 3-15 parts of CYMEL250 and 2-10 parts of CYMEL370N, preferably, the easy identification functional composition comprises 5-15 parts of CYMEL250 and 5-10 parts of CYMEL370N.

[0072] Furthermore, the silane coupling agent is a silane coupling agent containing a siloxy group, and its structure is usually represented by R-SiX3. Specifically, X represents a methoxy group or an ethoxy group, and R represents a functional group such as a thiol group, a polysulfide group, an amino group, a modified amino group, a vinyl group, an epoxy group, a cyano group, an isocyanate group, a methylvinyloxy group, etc., and is selected from one or a combination of KH-550, KH-560, KH-570, KH-580, KH-590, KH-902, KH-792, and KH-903 of Dow Corning. In a specific embodiment, the easy-to-identify functional composition contains 2 to 5 parts of a silane coupling agent.

[0073] Further, the auxiliary agent includes one or a combination of antioxidants, light aging agents and leveling dispersants; illustratively, the antioxidant is selected from BASF's B215; the light aging agent is selected from Lianlong's UV944; the leveling dispersant is selected from BYK Chemical's BYK-345, BYK-187, BYK-192 or a combination of several. In a specific embodiment, the auxiliary agent includes 1 to 5 parts of antioxidants, 1 to 5 parts of light aging agents and 1 to 5 parts of leveling dispersants. It should be understood by those skilled in the art that the auxiliary agent can be selected according to actual process requirements, and the scope of the auxiliary agents that can be used in the present invention is not limited to the auxiliary agents listed above.

[0074] The use of solvent is to better disperse the raw materials of the easily identifiable functional composition, and technicians can adjust it according to the actual raw material formula. In a specific embodiment, the solvent is selected from isooctyl alcohol and deionized water.

[0075] Furthermore, the metal primer of the present invention must contain a certain amount of effect pigments containing metal components such as aluminum powder, copper powder or nickel powder. These metal components in the metal primer need to be used to further reflect the laser penetrating the easy-to-identify layer. The technician can add special effect pigments such as pearlescent mica and glass powder, or infrared absorbing pigments, fillers, resins and other additives to the metal primer according to application needs, such as carbon black, graphene, carbon nanotubes and other carbon material pigments, cobalt blue, cobalt green blue-green pigments, iron oxide black pigments, etc. In addition, when spraying the metal substrate, for the present invention, the metal primer used has a strong covering power, so that the laser cannot penetrate the metal primer. In a specific embodiment, the metal primer is selected from Nippon Paint's AR3500 (T) silver primer, which is also applicable to primers of other colors.

[0076] The present invention also provides a method for preparing the composite coating as described above, comprising the following steps:

[0077] Spray metal primer on the surface of the substrate to obtain a base coat after the surface is dried;

[0078] Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried;

[0079] The coating is dried naturally or baked at room temperature to completely dry the base coating and the easy-to-identify layer to obtain a composite coating.

[0080] Furthermore, the easily identifiable functional composition is prepared according to the following steps:

[0081] Add the formulated amount of acrylic resin, amino resin and additives into the premixing container, mix well, add high refractive index micro beads, and disperse at high speed for 10 to 15 minutes;

[0082] Continue to add silane coupling agent and disperse at high speed for 5 to 10 minutes, add solvent and disperse at high speed for 5 to 10 minutes until uniform.

[0083] Furthermore, the rotation speed of the high-speed dispersion is 1000-1500 r / min.

[0084] Furthermore, the substrate is selected from a metal substrate or a non-metal substrate; the metal substrate is selected from tinplate or stainless steel; the non-metal substrate is selected from PP plastic board.

[0085] Furthermore, the baking condition is baking at 140-160° C. for 30-60 min.

[0086] Furthermore, the dry film thickness of the primer layer is 14 to 16 μm, and the dry film thickness of the easy-to-identify layer is 43 to 47 μm.

[0087] The specific embodiments of the present invention are described in detail below.

[0088] Example 1

[0089] This embodiment provides a formula of an easily identifiable functional composition, see Table 1.

[0090] Table 1 Easy-to-identify functional composition formula

[0091]

[0092]

[0093] This embodiment also provides a method for preparing a composite coating, comprising the following steps:

[0094] Add the formulated amount of acrylic resin, amino resin, antioxidant, light aging agent and leveling dispersant into a premixing container, mix well, add high refractive index microbeads, and disperse at high speed at 1000-1500 r / min for 10-15 minutes; continue to add silane coupling agent, disperse at high speed at 1000-1500 r / min for 5-10 minutes, add solvent, and disperse at high speed at 1000-1500 r / min for 5-10 minutes until uniform, to obtain an easily identifiable functional composition;

[0095] Spray AR3500(T) silver primer produced by Nippon Paint on the surface of the tinplate to obtain a base coat after the surface is dried;

[0096] Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried;

[0097] The samples were baked at 140°C for 40 minutes to completely dry the primer layer and the easy-to-identify layer, and finally a test sample was obtained, wherein the dry film thickness of the primer layer was about 15 μm, and the dry film thickness of the easy-to-identify layer was about 45 μm.

[0098] Example 2

[0099] This embodiment provides a formula of an easily identifiable functional composition, see Table 2.

[0100] Table 2 Easy-to-identify functional composition formula

[0101]

[0102] The preparation method of the composite coating according to Example 1 comprises the following steps:

[0103] preparing an easily identifiable functional composition;

[0104] Spray AR3500(T) silver primer produced by Nippon Paint on the surface of the tinplate to obtain a base coat after the surface is dried;

[0105] Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried;

[0106] The samples were baked at 140°C for 40 minutes to completely dry the primer layer and the easy-to-identify layer, and finally a test sample was obtained, wherein the dry film thickness of the primer layer was about 15 μm, and the dry film thickness of the easy-to-identify layer was about 45 μm.

[0107] Example 3

[0108] The formula of the easily identifiable functional composition used in this embodiment is the same as that in Embodiment 1, and the only difference from Embodiment 1 is that the material of the sprayed substrate is different.

[0109] The preparation method of the composite coating according to Example 1 comprises the following steps:

[0110] preparing an easily identifiable functional composition;

[0111] Spray AR3500(T) silver primer produced by Nippon Paint on the surface of the PP plastic plate, and obtain the base coating after the surface is dried;

[0112] Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried;

[0113] The samples were baked at 140°C for 40 minutes to completely dry the primer layer and the easy-to-identify layer, and finally a test sample was obtained, wherein the dry film thickness of the primer layer was about 15 μm, and the dry film thickness of the easy-to-identify layer was about 45 μm.

[0114] Example 4

[0115] The formula of the easily identifiable functional composition used in this embodiment is the same as that in Embodiment 2, and the only difference from Embodiment 2 is that the material of the sprayed substrate is different.

[0116] The preparation method of the composite coating according to Example 2 comprises the following steps:

[0117] preparing an easily identifiable functional composition;

[0118] Spray AR3500(T) silver primer produced by Nippon Paint on the surface of the PP plastic plate, and obtain the base coating after the surface is dried;

[0119] Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried;

[0120] The samples were baked at 140°C for 40 minutes to completely dry the primer layer and the easy-to-identify layer, and finally a test sample was obtained, wherein the dry film thickness of the primer layer was about 15 μm, and the dry film thickness of the easy-to-identify layer was about 45 μm.

[0121] Comparative Examples 1-6

[0122] This comparative example provides a test sample preparation scheme that was experimented during the research process. The formula of the easily identifiable functional composition and the type of substrate are shown in Table 3. The preparation method of the composite coating refers to Example 1, with the only difference being that the base coating is not sprayed on the surface of the substrate or a conventional primer is used instead of Nippon Paint's AR3500(T) silver primer.

[0123] Table 3 Easy-to-identify functional composition formula and substrate type

[0124]

[0125]

[0126] Note: The conventional primer coating is obtained by spraying Nippon Paint's FLEX700 gray primer on the substrate surface. The FLEX700 gray primer does not contain any metal components and has a dry film thickness of 15μm.

[0127] Performance Test 1: LiDAR Reflectivity Test

[0128] The test samples prepared in Examples 1-4 and Comparative Examples 1-6 were cured for 24 to 48 hours after drying, and then the laser radar signal reflection intensity test was performed. Velodyne 32-line laser radar (905nm) and NeuvitionTitan M1 laser radar (1550nm) were used to measure the reflection signal intensity at different incident angles at different distances, and the numerical value range was between 0-255.

[0129] See also Figure 1-Figure 3 ,in Figure 1 Schematic diagrams of the structures of different test samples are shown. It should be noted that when there is no primer layer, the structure of the test sample can be understood as a single-coating structure of substrate + easy-to-identify layer. When there is a primer layer, the structure of the test sample can be understood as a double-coating structure of substrate + metal primer / non-metal primer + easy-to-identify layer. Figure 2 This is a schematic diagram of the test sample being fixed on the sample test stand. Figure 3 The invention shows a reflection intensity testing method using a sample test stand and a laser radar device to simulate the change of incident angle.

[0130] The specific test methods are as follows:

[0131] (1) a sample test stand and a test sample are arranged at a fixed distance and height, the test sample is placed on the sample test stand, and the sample test stand can rotate around a fixed axis to change the incident angle of the laser;

[0132] (2) Setting up a laser radar bracket and a laser radar, wherein the laser radar is in the direction of the normal line of the plane where the sample test frame and the test sample are located, and is consistent with the level and height thereof;

[0133] (3) Turn on the Velodyne 32-line (signal source 905nm laser) laser radar and the PC device connected to it, run the supporting software VeloView test software to read the signal strength value of the test sample surface returned on the laser radar scanning data point cloud map, and take the average of the data point intensity of the entire board surface to obtain the reflected signal strength;

[0134] (4) Rotate the sample bracket around a fixed axis to gradually change the incident angle of the laser radar signal and record the reflected signal intensity at different incident angles;

[0135] (5) Replace the laser radar with a different signal source and repeat steps (3) and (4) using the Titan M1 (signal source 1550nm laser) laser radar. Test and record data in the same way. The results are shown in Table 4.

[0136] Table 4 Summary of LiDAR reflectivity test data

[0137]

[0138]

[0139] Result description:

[0140] The reflection intensity of Comparative Examples 1 and 4, which contain neither high-refractive microbeads nor primer, is weak, and the reflection intensity of PP plastic plate is weaker than that of tinplate; the reflection intensity of Comparative Examples 2 and 5 after adding high-refractive microbeads is significantly improved, showing the role of high-refractive microbeads in enhancing the reflection intensity; and the reflection intensity of Comparative Examples 3 and 6 after adding conventional primer is further improved, but Comparative Examples 1-6 still have the problem of strong angle sensitivity, and the reflection intensity at different incident angles fluctuates greatly. At the test distances of 3m and 7m, the maximum reduction in reflection intensity can reach more than 80%, which will seriously affect the acquisition and recognition of the lidar sensor.

[0141] On the other hand, the test samples prepared in Examples 1-4 of the present invention have significantly better test performance than the comparative examples. Taking the test sample prepared in Example 1 as an example, the aluminum powder flake structure contained in the AR3500 (T) silver primer further reflects the laser penetrating the easy-to-identify layer, so that the reflection intensity is further improved compared with the comparative example, and the synergistic enhancement effect of the high-refractive index microspheres and the metal primer is achieved. When the amount of glass microspheres added is moderately increased, the reflection intensity increases. At the same time, the fluctuation of the reflection intensity at different incident angles is significantly reduced. At the test distances of 3m and 7m, the maximum drop in its reflection intensity is no more than 27%, indicating that the composite coating of the present invention is conducive to the collection and identification of the laser radar sensor.

[0142] In addition, due to the strong hiding power of metal primer, the reflection intensity is equally strong regardless of whether it is a metal substrate (such as tinplate or stainless steel) or a non-metal substrate (such as PP plastic board). This is because the laser cannot penetrate the metal primer, and the material of the substrate will not affect the reflection performance.

[0143] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A composite coating that facilitates the acquisition and identification of laser radar sensors, characterized in that: It includes a base coat and a transparent or translucent easily identifiable layer sprayed thereon; The base coating is obtained by spraying a metal primer; The easy-to-identify layer is obtained by spraying an easy-to-identify functional composition, and the easy-to-identify functional composition includes the following raw materials in parts by weight: 15-60 parts of acrylic resin; 5-20 parts of amino resin; Silane coupling agent 0-5 parts; 15-45 parts of high refractive index micro beads; 1 to 10 parts of additives; 2 to 20 parts of solvent.

2. The composite coating according to claim 1, characterized in that: The high refractive index microbeads account for 15 to 45 wt% of the total weight of the easy-to-identify functional composition; Preferably, the refractive index of the high-refractive-index microbeads in the near-infrared spectral region is not less than 1.75; Preferably, the refractive index of the high-refractive-index microbeads in the near-infrared spectral region is not less than 1.9; Preferably, the refractive index of the high refractive index microbeads in the near infrared spectrum region is between 1.9 and 2.

7.

3. The composite coating according to claim 1, characterized in that: The particle size of the high refractive index microbeads is 0.01 to 350 μm; Preferably, the particle size of the high refractive index microbeads is 0.1-50 μm.

4. The composite coating according to claim 1, characterized in that: The high refractive index microspheres are selected from one or a combination of high refractive index glass microspheres, high refractive index optically transparent ceramic microspheres, and high refractive index amorphous polymer microspheres; Preferably, the high refractive index microspheres are selected from CX-1000 high refractive index glass microspheres produced by Weicaixiang Technology Co., Ltd.

5. The composite coating according to claim 1, characterized in that: The acrylic resin is selected from EMA-1032 and / or EMA-1015 of Nippon Paint Co., Ltd.; the amino resin is selected from CYMEL250 and / or CYMEL370N of Cytec Chemicals; The silane coupling agent is selected from one or a combination of KH-550, KH-560, KH-570, KH-580, KH-590, KH-902, KH-792 and KH-903 of Dow Corning; The auxiliary agent includes one or a combination of antioxidants, light aging agents and leveling dispersants.

6. The composite coating according to claim 5, characterized in that: The antioxidant is selected from BASF's B215; the light aging agent is selected from Lianlong's UV944; the leveling dispersant is selected from BYK-345, BYK-187, BYK-192 or a combination of several thereof.

7. The composite coating according to claim 1, characterized in that: The metal primer is selected from AR3500(T) silver primer produced by Nippon Paint.

8. The method for preparing the composite coating according to any one of claims 1 to 7, characterized in that: The steps include: Spraying a metal primer on the surface of the substrate to obtain a base coat after the surface is dried; Continue spraying the easily identifiable functional composition on the base coating to obtain an easily identifiable layer after the surface is dried; The coating is dried naturally or baked at room temperature to completely dry the base coating and the easy-to-identify layer to obtain a composite coating.

9. The preparation method according to claim 8, characterized in that: The substrate is selected from a metal substrate or a non-metal substrate; The metal substrate is selected from tinplate or stainless steel; the non-metal substrate is selected from PP plastic plate.

10. Application of the composite coating according to any one of claims 1 to 7 in intelligent automobile painting and intelligent robot painting.

Citation Information

Patent Citations

  • Laser radar diffuse reflection calibration plate

    CN114181618A

  • Coating system for surface of traffic facility or vehicle and preparation method thereof

    CN115873459A

  • Color-changing reflective paint surface of bicycle

    CN117143490A

  • Primer composition for optical article, and optical article

    JP2011219619A

  • Retroreflection sheet and outer type illumination system

    US20060256439A1