A high temperature resistant and oxidation resistant composite brazing material for alumina ceramics and a brazing method
By using composite solder materials of oxides such as Au and TiO2, the problem of poor welding performance in air reaction brazing of alumina ceramics is solved, and high-temperature stability and strength welding effects are achieved, which is suitable for a variety of welding scenarios and reduces the cost of Process complexity.
Patent Information
- Application Number
- CN202211462158.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-21
AI Technical Summary
The existing alumina ceramic air-reactive solder has poor overall performance during welding. The thickness of the welding layer and the welding temperature have a great impact on the welding effect, and it is difficult to maintain stability and strength in high temperature and oxygen-rich environments.
Composite solder prepared from Au, TiO2 and their coordinated oxides (SiO2, Fe2O3, Nb2O5, WO3) is pressed into solder sheets or slurries after rolling mixing and drying, and air reaction brazing is performed using a muffle furnace. Adjust welding temperature and pressure for stable welding.
The high-temperature stability and oxidation resistance of alumina ceramic welding parts are achieved, and the welding strength reaches more than 100MPa. It is suitable for welding of different structures and sizes, and reduces the complexity of the welding process and equipment requirements.
Smart Images

Figure CN115673603B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of brazing, and specifically relates to a high temperature resistant and oxidation resistant composite brazing material for alumina ceramics, a preparation method of the composite brazing material, and an air reaction brazing method for alumina ceramics. Background Art
[0002] Ceramic welding technologies include brazing, diffusion welding, instantaneous liquid phase connection, etc. Among them, the brazing method is convenient and flexible, with high production efficiency, and is applicable to both oxide and non-oxide ceramics. Ceramic brazing technologies include metallization brazing, active metal brazing, air reaction brazing, and auxiliary brazing such as ultrasonic, laser, and microwave. Compared with air reaction brazing, other brazing technologies are more complicated and have higher equipment requirements. For example, active metal brazing needs to be carried out under high vacuum or gas protection atmosphere, metallization brazing usually requires two major steps of high-temperature metallization and vacuum brazing (or atmosphere protection brazing), while air reaction brazing only needs to be heated in an ordinary muffle furnace. In particular, since the air reaction brazing filler metal is composed of a composite of antioxidant precious metals and oxides, the prepared brazed joints are used in oxygen-rich and high-temperature environments, and the joint strength is also high.
[0003] Based on the above advantages, air reaction brazing is the most commonly used welding process in ceramic welding. Different brazing materials are usually required for different types and uses of ceramics. For alumina ceramics, air reaction composite brazing materials mainly use Ag as the main metal and add a certain amount of metal oxides such as CuO, V2O5, CuO-B2O3, etc. For example, "Weil KS, et al. Oxidation ceramic to metal braze seals for applications in high temperature electrochemical devices and method of making," disclosed in U.S. Patent No. 10334346, and "Li Xinyue, et al. Mechanism of air reaction brazing of Al2O3 ceramics with Ag-CuO-B2O3 brazing material. Journal of the Chinese Ceramic Society, 2022, 50: 704-712."
[0004] In addition to Ag, these conventional brazing materials also use Pd and Pt as the main metal. For example, the document "Luo Y, et al. Reactive air brazing of Al2O3 ceramic with Ag-CuO-Pt composite fillers: microstructure and joint properties. Journal of the European Ceramic Society, 2021, 41: 1407–1414" discloses an Ag-Pd-CuO solution. In the published patent documents, there are also cases where the Pt-Nb2O5 system is applied to alumina ceramic brazing.
[0005] Most of the solders in the above schemes use Ag, Pd or Pt as the main metal, supplemented by some metal oxide as flux. The welding effect of the solders of these conventional schemes is usually not balanced, and it is impossible to meet the requirements in multiple aspects such as welding strength, oxidation resistance, high temperature resistance, and material expansion coefficient. For example, the thermal expansion coefficient of the main metal of the Ag-based solder is too high, the metal oxidation resistance of the Ag-Pd-based solder is insufficient during the air reaction brazing process, and the brazing temperature of the Pt-based solder is too high, the brazing temperature is ≥1800℃, which exceeds the tolerance temperature of ordinary ceramics.
[0006] In addition, most existing solders have strict requirements on the thickness of the solder layer and the soldering temperature. Too thick or too thin solder layer, or too high or too low soldering temperature may affect the soldering effect of the welded parts. This limits the application of solders on different welded parts and increases the difficulty of process control of the welding process. Summary of the invention
[0007] In order to solve the problems that the existing brazing materials have poor comprehensive performance during air reaction brazing of alumina ceramics, and the thickness of the welding layer and the welding temperature have a great influence on the welding effect, the present invention provides a high temperature resistant and oxidation-resistant composite brazing material for alumina ceramics, as well as a preparation method of the composite brazing material and an air reaction brazing method.
[0008] The present invention is implemented by the following technical solutions:
[0009] A high temperature resistant and oxidation resistant composite brazing material for alumina ceramics, the chemical composition of the composite brazing material includes Au, TiO2, and oxides for coordination; the oxides for coordination are selected from one or more of SiO2, Fe2O3, Nb2O5 and WO3. In the composite brazing material, the molar percentage of TiO2 is 0.5% to 1% according to the amount of substance; the total molar percentage of oxides is 4% to 20%; and the balance is Au.
[0010] As a further improvement of the present invention, applicable product forms of the composite solder include solder sheets and solder slurries; when used as solder sheets, the product only contains uniformly dispersed composite solder components, and when used as solder slurries, the product contains composite solder in powder form and an organic carrier in liquid form, and the composite solder is uniformly dispersed in the organic carrier.
[0011] The present invention also includes a method for preparing a solder sheet, comprising the following steps:
[0012] (1) According to the preset molar ratio, Au powder and selected ceramic powders of various oxides are mixed, and anhydrous ethanol is added as a dispersant, and the mixture is rolled and mixed at a speed of 60 r / min for at least 48 h.
[0013] (2) The mixed material from the above step is taken out and placed in an oven, and dried at a temperature of 100 to 150° C. for 30 to 60 minutes to remove the anhydrous ethanol therein.
[0014] (3) Grind the dried solids again into a uniform powder.
[0015] (4) Using a hydraulic press at a pressure of 150-200 MPa, the uniform powder obtained in the previous step is pressed into a thin sheet with a thickness of 80-200 μm to obtain the desired solder sheet.
[0016] As a further improvement of the present invention, among the raw materials used for preparing the solder sheet, Au powder is selected to have a particle size of micrometer level or below; the purity of ceramic powders of various oxides is ≥99.9%; and the thickness of the prepared solder sheet is 80-200μm.
[0017] The present invention also includes a method for preparing a solder slurry, comprising the following steps:
[0018] (1) According to the preset molar ratio, Au powder and selected ceramic powders of various oxides are placed in a rolling ball mill, and anhydrous ethanol is added as a dispersant, and the mixture is rolled and mixed at a speed of 60 r / min for at least 48 h.
[0019] (2) The mixed material from the above step is taken out and placed in an oven, and dried at a temperature of 100 to 150° C. for 30 to 60 minutes to remove the anhydrous ethanol therein.
[0020] (3) Grind the dried solids again into a uniform powder.
[0021] (4) Preparing a uniformly dispersed liquid organic carrier according to the preset components and ratios.
[0022] (5) The uniform powder of step (3) and the liquid organic carrier of step (4) are mixed according to a preset mass ratio to prepare a uniformly dispersed slurry, which is the desired solder slurry.
[0023] As a further improvement of the present invention, in step (1), the Au powder is selected to have a particle size of micrometer level or below; and the purity of the ceramic powders of various oxides is ≥99.9%.
[0024] In step (4), the components of the organic carrier include, by mass percentage, 86 wt.% terpineol, 8 wt.% ethyl cellulose, 2 wt.% hydrogenated castor oil, 2 wt.% Span 85 and 2 wt.% 1,4-butyrolactone.
[0025] The mass ratio of the uniform powder and the liquid organic carrier in the preparation process of step (5) is 1:1.
[0026] The present invention also includes an air reaction brazing method for alumina ceramics, which is used to braze two weldments made of the same alumina ceramics; the air reaction brazing method includes the following steps:
[0027] (1) Grind and polish the welding surfaces of the two alumina ceramic weldments to be welded.
[0028] (2) The entire polished alumina ceramic substrate or the portion including the welding surface is placed in a weak alkaline solution and boiled for 30 minutes.
[0029] (3) The alumina ceramic substrate after the alkali treatment in the above step is washed with water and then dried in an oven.
[0030] (4) Cutting the solder sheet prepared by the above-mentioned method for preparing the solder sheet into a shape and size that matches the welding surface.
[0031] (5) Place the brazing material sheet between the welding surfaces of the two welds, apply a pressure of 10 to 20 kPa to the welds, heat treat at a temperature of 1200 to 1600°C for 5 to 60 minutes, and then cool to room temperature to complete the brazing of the welds.
[0032] The present invention also includes an air reaction brazing method for alumina ceramics, which is used to braze two weldments made of the same alumina ceramics; the method specifically includes the following steps:
[0033] (1) Grind and polish the welding surfaces of the two alumina ceramic weldments to be welded.
[0034] (2) The entire polished alumina ceramic substrate or the portion including the welding surface is placed in a weak alkaline solution and boiled for 30 minutes.
[0035] (3) The alumina ceramic substrate after the alkali treatment in the above step is washed with water and then dried in an oven.
[0036] (4) A solder paste prepared by the method for preparing solder paste as described in claim 5; the solder paste is respectively printed on the welding surfaces of two weldments by screen printing, and the solder paste is dried.
[0037] (5) The welding surfaces containing the brazing material slurry in the two welds are placed face to face, a pressure of 10 to 20 kPa is applied to the welds, and heat treatment is performed at a temperature of 1200 to 1600°C for 5 to 60 minutes, and then cooled to room temperature to complete the brazing of the welds.
[0038] As a further improvement of the present invention, the thickness of the solder paste printed on the welding surface of the weldment is 10 to 40 μm.
[0039] In the above two different air reaction brazing methods, the welding process of the assembled parts to be welded is detailed as follows:
[0040] First, place the workpiece to be welded in a muffle furnace and apply a micro-pressure of 10 to 20 kPa to the weldment through a pressing block; then, increase the furnace temperature to a brazing temperature of 1200 to 1600°C at a heating rate not exceeding 10°C / min, and perform heat treatment at this temperature for 5 to 60 minutes; then, reduce the furnace temperature to 500°C at a cooling rate of 5°C / min; finally, cool the welded product to room temperature with the furnace and take it out; brazing is completed.
[0041] The technical solution provided by the present invention has the following beneficial effects:
[0042] The composite brazing material provided by the present invention has a close thermal expansion coefficient to that of alumina ceramics, and the two materials can form a stable interface effect at high temperature, so it can be used as a brazing material for alumina ceramic substrates. When the composite brazing material is used for brazing alumina ceramics, the room temperature welding strength reaches more than 100MPa; and it has high high temperature resistance and thermal shock resistance.
[0043] The formula of the composite brazing material provided by the present invention mainly includes the main metal material Au and two types of oxide materials, and each material component is a high melting point material, so when used for brazing alumina ceramics, a welding layer structure with extremely strong high temperature resistance and oxidation resistance can be produced. This allows the alumina ceramic welded parts to work stably for a long time in a harsh environment of high temperature, oxygen-rich, and even high-frequency vibration.
[0044] The composite brazing material provided by the present invention has a wide range of uses and can be applied to the brazing connection between alumina ceramic structures of different structures and sizes. In addition, the requirements for the welding process are relatively low, and the air reaction brazing of the weldment can be completed using a conventional muffle furnace. At the same time, the composite brazing material can achieve a relatively good welding effect in a relatively wide brazing temperature range of 1200 to 1600° C., and has a relatively strong process adaptability.
[0045] In summary, the composite brazing material provided in this embodiment is a high-temperature resistant and oxidation-resistant brazing material specially used for alumina ceramics, has very excellent and comprehensive comprehensive performance, and has high practical value. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a flow chart of the method for preparing the solder sheet provided in Example 1 of the present invention.
[0047] Figure 2 This is a flow chart of the method for preparing the solder slurry provided in Example 1 of the present invention.
[0048] Figure 3 This is a process flow chart for brazing alumina ceramics using brazing slurry according to Example 2 of the present invention.
[0049] Figure 4 This is a process flow chart for brazing alumina ceramics using brazing sheets according to Example 2 of the present invention. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0051] Example 1
[0052] This embodiment provides a high temperature resistant and anti-oxidation composite brazing material for alumina ceramics, the chemical composition of the composite brazing material includes Au, TiO2, and oxides for coordination; the oxides for coordination are selected from one or more of SiO2, Fe2O3, Nb2O5 and WO3. In the composite brazing material, the molar percentage of TiO2 is 0.5% to 1% according to the amount of substance; the total molar percentage of oxides is 4% to 20%; and the balance is Au.
[0053] In the brazing material formula of this embodiment, the main metal is Au; the thermal expansion performance of Au is relatively matched with that of alumina ceramics, and it has a wide brazing temperature range, and the material of Au itself has good high temperature resistance and oxidation resistance. Therefore, the use of Au as the main metal in this embodiment is the basis for improving the welding effect of alumina ceramic weldments, and ensures that the welding layer has better high temperature resistance and oxidation resistance.
[0054] The solder formula of this embodiment selects two types of high melting point oxide materials with different properties as flux for the main metal. One of them is TiO2, which is mainly used in the formula of this embodiment to improve the interface effect between the solder layer and the alumina ceramic matrix in the two welds after welding, and significantly improve the welding strength. The other is a specially selected oxide ceramic material, which includes SiO2, Fe2O3, Nb2O5 and WO3. The addition of these components can further adjust the overall thermal expansion coefficient of the solder, making the thermal expansion coefficient of the solder layer and the weld closer.
[0055] In particular, after adding the oxides of the above components in a specific ratio in this embodiment, the range of the welding temperature of the weldment can be significantly widened. Through experimental verification, it is found that within a wide temperature range of 1200-1600°C, a better welding effect can be achieved for alumina ceramics, which shows that the brazing material can reduce the influence of the welding temperature on the welding quality of the weldment.
[0056] Another outstanding advantage of the composite solder with a specific formula provided in this embodiment is its good adaptability to various brazing processes and different welding scenarios. Whether a thinner (20-80 μm) solder layer thickness or a thicker (80-200 μm) solder layer thickness is used, the composite solder can maintain a high welding quality, and even if the solder layer thickness reaches more than 150 μm, a relatively dense solder layer can still be formed; this allows the solder to be used for brazing large-sized weldments and ultra-thin micro weldments at the same time. The welding process only requires a simple muffle furnace, without the need for vacuum or special atmosphere protection, and has lower requirements for the welding process and more relaxed restrictions on process parameters.
[0057] Based on the above advantages, the applicable product forms of the composite solder of the specific formula provided in this embodiment include solder sheets and solder slurry. When used as solder sheets, the product only contains uniformly dispersed composite solder components. This type of product is mainly used for welding larger weldments, and the thickness of the solder sheet is 80 to 200 μm.
[0058] When used as solder paste, the product contains a composite solder in powder form and a liquid organic carrier, and the composite solder is evenly dispersed in the organic carrier. This solder product can be used for welding thinner micro-welds. When the solder is applied by screen printing, the thickness of the solder layer can be as low as about 20μm.
[0059] Specifically, this embodiment provides a method for preparing this type of solder sheet, such as Figure 1 As shown, the specific steps include:
[0060] (1) According to the preset molar ratio, Au powder and selected ceramic powders of various oxides are placed in a rolling ball mill, and anhydrous ethanol is added as a dispersant, and the mixture is rolled and mixed at a speed of 60 r / min for at least 48 h.
[0061] (2) The mixed material from the above step is taken out and placed in an oven, and dried at a temperature of 100 to 150° C. for 30 to 60 minutes to remove the anhydrous ethanol therein.
[0062] (3) Grind the dried solids again into a uniform powder.
[0063] (4) Using a hydraulic press at a pressure of 150-200 MPa, the uniform powder obtained in the previous step is pressed into a thin sheet with a thickness of 80-200 μm to obtain the desired solder sheet.
[0064] Among the raw materials used for preparing the solder sheet, Au powder is selected to have a particle size of micrometer level or below; the purity of ceramic powders of various oxides is ≥99.9%.
[0065] Accordingly, if Figure 2 As shown, the preparation method of the aforementioned solder slurry comprises the following steps:
[0066] (1) According to the preset molar ratio, Au powder and selected ceramic powders of various oxides are placed in a rolling ball mill, and anhydrous ethanol is added as a dispersant, and the mixture is rolled and mixed at a speed of 60 r / min for at least 48 h.
[0067] Among them, Au powder is selected to have a particle size of micron level or below; the purity of ceramic powders of various oxides is ≥99.9%.
[0068] (2) The mixed material from the above step is taken out and placed in an oven, and dried at a temperature of 100 to 150° C. for 30 to 60 minutes to remove the anhydrous ethanol therein.
[0069] (3) Grind the dried solids again into a uniform powder.
[0070] (4) Preparing a uniformly dispersed liquid organic carrier according to the preset components and ratios.
[0071] (5) The uniform powder of step (3) and the liquid organic carrier of step (4) are mixed according to a preset mass ratio to prepare a uniformly dispersed slurry, which is the desired solder slurry.
[0072] It should be noted that in the solder paste, the organic carrier generally includes a variety of functional additives such as dispersants, antioxidants, anticoagulants, thickeners, defoamers, etc. The composite paste provided in this embodiment has no special restrictions on the composition and type of the organic carrier when preparing the solder paste, and various conventional formulas can be used.
[0073] In addition, in order to be applied to different scenarios, technicians can also reasonably adjust the ratio of the composite solder and the organic carrier according to the requirements for the solder concentration and viscosity of the solder slurry. For example, in this embodiment, the components of the organic carrier used, by mass percentage, include 86wt.% pine alcohol, 8wt.% ethyl cellulose, 2wt.% hydrogenated castor oil, 2wt.% Span 85 and 2wt.% 1,4-butyrolactone. The mass ratio of the powder and liquid organic carrier in the modulation process is 1:1.
[0074] Example 2
[0075] This embodiment provides a welding process for welding alumina ceramics using the composite brazing filler metal in Embodiment 1. Depending on the type of alumina ceramic weldment, different types of composite brazing filler metal products may be used and different welding processes may be used for welding.
[0076] Among them, for conventional alumina ceramic weldments with thicker materials and larger volumes, the brazing sheet in Example 1 is preferably selected as the welding material, and the following is used: Figure 3 The following welding methods are shown:
[0077] (1) Grind and polish the welding surfaces of the two alumina ceramic weldments to be welded.
[0078] (2) The entire polished alumina ceramic substrate or the portion including the welding surface is placed in a weak alkaline solution and boiled for 30 minutes.
[0079] (3) The alumina ceramic substrate after the alkali treatment in the above step is washed with water and then dried in an oven.
[0080] (4) Cut the solder sheet into a shape and size that matches the welding surface.
[0081] (5) Place the brazing material sheet between the welding surfaces of the two welds, apply a pressure of 10 to 20 kPa to the welds, heat treat at a temperature of 1200 to 1600°C for 5 to 60 minutes, and then cool to room temperature to complete the brazing of the welds.
[0082] Among them, for the micro-alumina ceramic weldment with relatively light and thin materials and small volume, the brazing material slurry in Example 1 is preferably selected as the welding material, and the following is used: Figure 4 The following welding methods are shown:
[0083] (1) Grind and polish the welding surfaces of the two alumina ceramic weldments to be welded.
[0084] (2) The polished alumina ceramic substrate is placed in a weak alkaline solution and boiled for 30 minutes.
[0085] (3) The alumina ceramic substrate after the alkali treatment in the above step is washed with water and then dried in an oven.
[0086] (4) Print the solder paste onto the welding surfaces of the two weldments by screen printing, and dry the solder paste.
[0087] During the screen printing process, the thickness of the solder paste on the two welds is set to half of the overall thickness. Specifically, the thickness of the solder paste printed on the welding surface of a single weld is 10-40 μm.
[0088] (5) The welding surfaces containing the brazing material slurry in the two welds are placed face to face, a pressure of 10 to 20 kPa is applied to the welds, and heat treatment is performed at a temperature of 1200 to 1600°C for 5 to 60 minutes, and then cooled to room temperature to complete the brazing of the welds.
[0089] In the above two different air reaction brazing methods, the welding process of the assembled parts to be welded is detailed as follows:
[0090] First, place the workpiece to be welded in a muffle furnace, and apply a micro-pressure of 10 to 20 kPa to the weldment through a press block or other means as needed. Then, raise the furnace temperature to a brazing temperature of 1200 to 1600 °C at a heating rate not exceeding 10 °C / min, and heat treat for 5 to 60 minutes. Next, lower the furnace temperature to 500 °C at a cooling rate of 5 °C / min. Finally, cool the welded product to room temperature with the furnace and take it out; brazing is completed.
[0091] Performance Testing
[0092] In order to verify the various properties of the composite brazing material provided by this embodiment, as well as the welding effect of the composite brazing material on different types of alumina ceramics, samples of the composite brazing material are first trial-produced during the performance testing phase, and then different types of weldments are welded using different processes, and finally the welding quality of the weldments after welding is tested.
[0093] 1. Sample production of composite solder
[0094] During this test, a total of 5 composite solder samples were trial-produced, including 3 different solder paste type samples and 2 different solder sheet type samples. Among them, when preparing the solder paste, the organic carrier used is a pre-prepared solvent-based organic carrier containing 86wt.% pine alcohol, 8wt.% ethyl cellulose, 2wt.% hydrogenated castor oil, 2wt.% Span 85 and 2wt.% 1,4-butyrolactone. When the powder and organic paste are evenly dispersed, the solder paste is paste-like.
[0095] (1) Brazing slurry 1
[0096] The commercially available Au, SiO2 and TiO2 powders with molar percentages of 89.5%, 10% and 0.5% were placed in a rolling ball mill, anhydrous ethanol was used as a dispersant, and the mixture was rolled at a speed of 60r / min for 48 hours. The mixture was taken out and placed in an oven at 100°C for 60 minutes for drying, and then ground into a uniform powder. Finally, the mixed powder with a mass ratio of 1:1 and the above-mentioned organic carrier were prepared into a composite solder slurry.
[0097] (2) Brazing material slurry 2
[0098] The commercially available Au, Fe2O3 and TiO2 powders with molar percentages of 79%, 20% and 1% were placed in a rolling ball mill, anhydrous ethanol was used as a dispersant, and the mixture was rolled at a speed of 60r / min for 48 hours. The mixture was taken out and placed in an oven at 150°C for 60 minutes for drying, and then ground into a uniform powder. Finally, the mixed powder with a mass ratio of 1:1 and the above-mentioned organic carrier were prepared into a composite solder slurry.
[0099] (3) Brazing slurry 3
[0100] According to the molar percentage, 91.5% of commercially available Au, 8% of an equal ratio mixture of Nb2O5 and WO3, and 0.5% of TiO2 powder were placed in a rolling ball mill, anhydrous ethanol was used as a dispersant, and the mixture was rolled at a speed of 60r / min for 48 hours, taken out and placed in an oven at 100°C, kept warm for 60 minutes to dry, and then ground into a uniform powder. Finally, the mixed powder with a mass ratio of 1:1 and the above-mentioned organic carrier were prepared into a composite solder slurry.
[0101] (4) Solder sheet 1
[0102] According to the molar percentage, 95.5% of commercially available Au, 0.5% of TiO2 powder, and 1% of SiO2, Fe2O3, Nb2O5 and WO3 powder were placed in a rolling ball mill, with anhydrous ethanol as a dispersant, and rolled at a speed of 60r / min for 48 hours, taken out and placed in an oven at 100°C, kept warm for 60 minutes to dry, and then ground into a uniform powder. The above powder was pressed into a composite solder sheet with a thickness of 200μm using a hydraulic press at a pressure of 200MPa.
[0103] (5) Solder sheet 2
[0104] Commercially available Au, WO3 and TiO2 powders with molar percentages of 95.5%, 4% and 0.5% respectively are placed in a rolling ball mill, with anhydrous ethanol as a dispersant, and rolled at a speed of 60r / min for 48 hours. The powders are taken out and placed in an oven at 100°C, kept warm for 60 minutes for drying, and then ground into uniform powder. A hydraulic press is used to press the above powders into a composite solder sheet with a thickness of 80μm at a pressure of 150MPa.
[0105] 2. Welding test of alumina ceramics
[0106] In the welding test of this embodiment, the weldments used mainly include three categories: one is a square alumina ceramic block with a length, width and height of 10mm×5mm×5mm respectively; one is a long strip of alumina ceramic with a length, width and height of 15mm×4mm×3mm respectively; and the other is an alumina ceramic sheet with a thickness of 3mm and a diameter of 20mm.
[0107] Among them, test example 1 uses brazing paste 1 to weld two alumina ceramic sheets. Test example 2 uses brazing paste 2 to perform side butt welding on two square ceramic blocks. Test example 3 uses brazing paste 3 to perform end-to-end welding on two long strips of alumina ceramics; and test example 4 selects brazing sheet 1 to perform side butt welding on two square alumina ceramic blocks. Test example 5 selects brazing sheet 2 to perform end-to-end welding on two long strips of alumina ceramics. The specific welding process is as follows:
[0108] (6) Brazing Test Example 1
[0109] First, the connection surface of the alumina ceramic to be welded is ground and polished on a precision grinding and polishing machine, and then boiled in a weak alkaline solution for 30 minutes, then rinsed with water, and finally dried in an oven.
[0110] Then, the solder paste 1 was screen-printed twice on the connection surface with a thickness of 10 μm, and placed in an oven at 150° C. for 30 minutes for drying.
[0111] Next, two pieces of alumina ceramics with composite brazing material coatings on their connection surfaces are placed face to face and placed in a muffle furnace, and then an additional pressure of 10 kPa is applied.
[0112] Finally, the furnace temperature was raised to the brazing temperature of 1600°C at a heating rate not higher than 10°C / min, the holding time was 5 minutes, and then the temperature was lowered to 500°C at a cooling rate of 5°C / min, and then cooled in the furnace.
[0113] (7) Brazing Test Example 2
[0114] First, the connection surface of the alumina ceramic to be welded is ground and polished on a precision grinding and polishing machine, and then boiled in a weak alkaline solution for 30 minutes, then rinsed with water, and placed in an oven at 100°C for 60 minutes for drying.
[0115] Then, the solder paste 2 was screen-printed 6 times on the connection surface with a thickness of 25 μm, and placed in an oven at 150° C. for 30 minutes for drying.
[0116] Next, two pieces of alumina ceramics with composite brazing slurry on the connection surfaces are placed face to face and placed in a muffle furnace, and then an additional pressure of 15 kPa is applied.
[0117] Finally, the temperature is raised to the brazing temperature of 1550°C at a heating rate not higher than 10°C / min, the holding time is 20 minutes, and then the temperature is lowered to 500°C at a cooling rate of 5°C / min, and then cooled in the furnace.
[0118] (8) Brazing Test Example 3
[0119] First, the connection surface of the alumina ceramic to be welded is ground and polished on a precision grinding and polishing machine, and then boiled in a weak alkaline solution for 30 minutes, then rinsed with water, and finally dried in an oven.
[0120] Then, the solder paste 3 was screen-printed 10 times on the connection surface with a thickness of 40 μm, and placed in an oven at 150° C. for 30 minutes for drying.
[0121] Next, two pieces of alumina ceramics with composite brazing material coatings on the connection surfaces are placed face to face and placed in a muffle furnace, and then an additional pressure of 20 kPa is applied.
[0122] Finally, the temperature is raised to the brazing temperature of 1500°C at a heating rate not higher than 10°C / min, the holding time is 30 minutes, and then the temperature is lowered to 500°C at a cooling rate of 5°C / min, and then cooled in the furnace.
[0123] (9) Brazing Test Example 4
[0124] First, the connection surface of the alumina ceramic to be welded is ground and polished on a precision grinding and polishing machine, and then boiled in a weak alkaline solution for 30 minutes, then rinsed with water, and placed in an oven at 100°C for 60 minutes for drying.
[0125] Next, the brazing sheet 1 is cut according to the size of the connection surface; the cut brazing sheet is placed between the two processed alumina ceramics; the assembled welded parts are placed in a muffle furnace, and then an additional pressure of 10 kPa is applied.
[0126] Finally, the temperature is raised to the brazing temperature of 1400°C at a heating rate not higher than 10°C / min, the holding time is 30 minutes, and then the temperature is lowered to 500°C at a cooling rate of 5°C / min, and then cooled in the furnace.
[0127] (10) Brazing Test Example 4
[0128] First, the connection surface of the alumina ceramic to be welded is ground and polished on a precision grinding and polishing machine, and then boiled in a weak alkaline solution for 30 minutes, then rinsed with water, and placed in an oven at 100°C for 60 minutes for drying.
[0129] Next, the brazing sheet 2 is cut according to the size of its connection surface; the cut composite brazing sheet is placed between the two alumina ceramics treated as above, and placed in a muffle furnace, and then an additional pressure of 20 kPa is applied.
[0130] Finally, the temperature is raised to the brazing temperature of 1200°C at a heating rate not higher than 10°C / min, the holding time is 60 minutes, and then the temperature is lowered to 500°C at a cooling rate of 5°C / min, and then cooled in the furnace.
[0131] 3. Welding quality test
[0132] This experiment designed the test tasks of room temperature shear strength and high temperature three-point bending strength respectively to test the welding interface strength of the brazed connectors of the corresponding composite brazing materials at room temperature and high temperature. Among them, the brazed connectors of test examples 2 and 4 are side-welded and used for room temperature shear strength tests. The brazed connectors of test examples 3 and 5 are side-welded and used for high temperature three-point bending strength tests. For test example 1, since a thin sheet substrate is used in the brazed connector, the above two test methods cannot be used to test the strength of the welded joint.
[0133] The test methods for the two test items are as follows:
[0134] (1) Room temperature shear strength
[0135] The test method for room temperature shear strength test of welded joints can be performed according to the method in the reference (Gui XY, et al, Experimental and theoretical study on air reaction wetting and brazing of Si3N4 ceramic by Ag-CuO filler metal: Performance and interfacial behaviorJournal of the European Ceramic Society, 2022, 42: 432–441).
[0136] (2) High temperature three-point bending strength
[0137] The high temperature strength of the welded joint was tested using a three-point bending test method, with a bending moment of 26 mm and a test temperature of 700 °C.
[0138] The test results of the room temperature shear strength and high temperature three-point bending strength of the brazed connection in Test Example 2-5 are shown in the following table:
[0139] Table 1: Test results of welded joint strength of brazed connections in different test cases
[0140]
[0141]
[0142] Analysis of the test data in the above table shows that: under different brazing material types and thicknesses, when the brazing material provided in this embodiment is used for alumina ceramic welding, the shear strength of the joint of the material exceeds 115MPa, which is higher than the welding strength requirements of various devices in the actual application of alumina ceramics. At the same time, under high temperature conditions, the three-point bending strength measured for each sample is higher than 70MPa, which reflects that the solder layer produced by the brazing material provided in this embodiment has strong high temperature resistance.
[0143] Combined with the above tests, it can be seen that the composite brazing filler metal provided in this embodiment can be used to weld different types of weldments, and for different brazing application scenarios, two different product forms of brazing filler metal slurry and brazing sheet can be used. When the composite brazing filler metal provided in this embodiment is used to weld an alumina substrate, within the range of 20-200 μm of the weld layer thickness, a welding effect that exceeds that of existing air-reactive brazing fillers can be achieved.
[0144] In addition, when the composite brazing material provided in this embodiment is used for brazing alumina ceramic materials, the interface effect between the materials is good because the thermal expansion coefficients between the welding layer and the material layer are close; the obtained brazed connector has outstanding high temperature resistance and thermal shock resistance. The components of the composite brazing material are all high temperature resistant and oxidation resistant materials, so the brazed connector can work in harsh environments with rich oxygen and high temperature, and has extremely high practical value.
[0145] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high temperature resistant and oxidation resistant composite brazing material for alumina ceramics, characterized in that: The chemical composition of the composite solder includes Au, TiO2, and oxides for coordination, wherein the oxides for coordination are selected from one or more of SiO2, Fe2O3, Nb2O5 and WO3; in the composite solder, the molar percentage of TiO2 is 0.5% to 1% based on the amount of substance; the total molar percentage of oxides is 4% to 20%; and the balance is Au; The high temperature resistant and oxidation resistant composite brazing agent for alumina ceramics is used to realize brazing connection between alumina ceramics, and the welding process is as follows: First, place the workpiece to be welded in a muffle furnace and apply a micro-pressure of 10~20kPa to the weldment; then, increase the furnace temperature to the brazing temperature of 1200~1600℃ at a heating rate not exceeding 10℃ / min, and keep the heat treatment for 5~60min; then, reduce the furnace temperature to 500℃ at a cooling rate of 5℃ / min; finally, cool the welded product to room temperature with the furnace and take it out; the brazing is completed.
2. The high temperature resistant and oxidation resistant composite brazing material for alumina ceramics according to claim 1, characterized in that: The applicable product forms of the composite solder include solder sheets and solder slurries; when used as solder sheets, the product only contains uniformly dispersed composite solder components; when used as solder slurries, the product contains composite solder in powder form and an organic carrier in liquid form, and the composite solder is uniformly dispersed in the organic carrier.
3. A method for preparing a solder sheet as claimed in claim 2, characterized in that: The steps include: (1) According to the preset molar ratio, Au powder and various selected oxide ceramic powders are mixed, and anhydrous ethanol is added as a dispersant, and the mixture is rolled and mixed at a speed of 60 r / min for at least 48 hours; (2) The mixed material from the previous step is taken out and placed in an oven, and dried at a temperature of 100-150° C. for 30-60 minutes to remove the anhydrous ethanol therein; (3) Grinding the dried solids into uniform powder again; (4) Use a hydraulic press at a pressure of 150-200 MPa to press the uniform powder from the previous step into thin sheets to obtain the required solder sheets.
4. The method for preparing a solder sheet according to claim 3, wherein: Among the raw materials used for preparing the solder sheet, the Au powder is selected to have a particle size of micrometer level or below; the purity of the ceramic powder of various oxides is ≥99.9%; and the thickness of the prepared solder sheet is 80-200 μm.
5. A method for preparing a solder slurry as claimed in claim 2, characterized in that: The steps include: (1) According to the preset molar ratio, Au powder and various selected oxide ceramic powders are placed in a rolling ball mill, and anhydrous ethanol is added as a dispersant, and the mixture is rolled at a speed of 60 r / min for at least 48 h; (2) The mixed material from the previous step is taken out and placed in an oven, and dried at a temperature of 100-150° C. for 30-60 minutes to remove the anhydrous ethanol therein; (3) Grinding the dried solids into uniform powder again; (4) preparing a uniformly dispersed liquid organic carrier according to the preset components and ratios; (5) The uniform powder of step (3) and the liquid organic carrier of step (4) are mixed in a preset mass ratio to form a uniformly dispersed slurry, which is the desired solder slurry.
6. The method for preparing the solder slurry according to claim 5, characterized in that: The Au powder in step (1) is selected to have a particle size of micrometer level or below; the purity of the ceramic powder of various oxides is ≥99.9%; In step (4), the components of the organic carrier include terpineol, ethyl cellulose, hydrogenated castor oil, Span 85 and 1,4-butyrolactone; The mass ratio of the uniform powder and the liquid organic carrier in the preparation process of step (5) is 1:
1.
7. An air reaction brazing method for alumina ceramics, which is used to braze two weldments made of the same alumina ceramics; characterized in that: The air reaction brazing method comprises the following steps: (1) Grinding and polishing the welding surfaces of the two alumina ceramic weldments to be welded; (2) The entire polished alumina ceramic substrate or the portion including the welding surface is placed in a weak alkaline solution and boiled for 30 minutes; (3) washing the alumina ceramic substrate after the alkali treatment in the above step with water, and then drying it in an oven; (4) cutting the solder sheet prepared by the method for preparing a solder sheet as claimed in claim 3 into a shape and size matching the welding surface; (5) Place the brazing material sheet between the welding surfaces of the two welded parts, place the welded parts in a muffle furnace, and apply a micro-pressure of 10-20 kPa to the welded parts; then, increase the furnace temperature to the brazing temperature of 1200-1600 °C at a heating rate not exceeding 10 °C / min, and heat treat for 5-60 min; then, reduce the furnace temperature to 500 °C at a cooling rate of 5 °C / min; finally, cool the welded product to room temperature with the furnace and take it out; the brazing is completed.
8. An air reaction brazing method for alumina ceramics, which is used to braze two weldments made of the same alumina ceramics; characterized in that: The air reaction brazing method comprises the following steps: (1) Grinding and polishing the welding surfaces of the two alumina ceramic weldments to be welded; (2) The entire polished alumina ceramic substrate or the portion including the welding surface is placed in a weak alkaline solution and boiled for 30 minutes; (3) washing the alumina ceramic substrate after the alkali treatment in the above step with water, and then drying it in an oven; (4) A solder paste prepared by the method for preparing a solder paste as claimed in claim 5; printing the solder paste on the welding surfaces of two welding parts respectively by screen printing, and drying the solder paste; (5) The welding surfaces containing the brazing slurry in the two weldments are placed face to face, and the weldments are placed in a muffle furnace. A micro-pressure of 10-20 kPa is applied to the weldments. Then, the furnace temperature is raised to a brazing temperature of 1200-1600°C at a heating rate not exceeding 10°C / min, and the heat treatment is carried out at this temperature for 5-60 min. Next, the furnace temperature is lowered to 500°C at a cooling rate of 5°C / min. Finally, the welded product is cooled to room temperature in the furnace and taken out. The brazing is completed.
9. The air reaction brazing method of alumina ceramics according to claim 8, characterized in that: The thickness of the solder paste printed on the welding surface of the weldment is 10~40μm.
Citation Information
Patent Citations
Real-time multivariable biometric analysis and display system and method
US10334346B2
Gold-based solder for connecting Al2O3 ceramics and metal and welding method thereof
CN108422058A
Brazing material and brazing method used for air atmosphere brazing of SiC ceramics
CN109822260A
Brazing filler metal and preparation method and brazing method thereof
CN115178913A
Brazing filler metal for joining ceramics and metal and its joining method
JP1993261588A