A laminated aluminum alloy composite plate and preparation method thereof

Through the homogenization and surface treatment of the panels, middle panels, and back panels, as well as high-temperature preheating, rolling, and online quenching treatments, the complexity and high cost of manufacturing layered composite armor materials are solved, and the lamination efficiency is significantly improved. The interface strength and interlayer bonding force of aluminum alloy composite plates achieve excellent mechanical properties and simplified process flow.

CN115674813BActive Publication Date: 2024-10-22JIMEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211465418.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-10-22
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

The existing layered composite armor materials have complex manufacturing technology, high cost and poor inter-layer bonding force, making it difficult to simultaneously improve the anti-elastic performance and protective capabilities of armored vehicles.

Method used

The preparation method of laminated aluminum alloy composite plates is adopted, including homogenization and surface treatment of panels, middle plates and back plates, preheating, rolling and online quenching after lamination, and finally aging treatment to improve interface strength. and interlayer bonding force.

Benefits of technology

It achieves the rapid preparation of laminated aluminum alloy composite plates with high interface bonding strength, simplifies the process flow, improves the mechanical properties and interlayer bonding strength, reduces production costs, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115674813B_ABST
    Figure CN115674813B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of preparation and processing of metal composite materials, and the present invention provides a laminated aluminum alloy composite plate and a preparation method thereof. The preparation method comprises the following steps: homogenizing the face plate, the middle plate and the back plate; performing surface treatment on the face plate, the middle plate and the back plate; combining the treated plates into a composite plate in the order of the face plate, the middle plate and the back plate, and riveting the front and rear ends with rivets; rapidly performing large deformation composite rolling on the composite plate after high temperature preheating treatment, and performing online quenching of the composite plate by strong air cooling or water quenching in the final rolling, and then performing aging treatment. High temperature large deformation composite rolling improves the interface strength of the laminated aluminum alloy composite plate, and the rolling online quenching eliminates the conventional artificial solid solution process, shortens the process flow, is highly efficient, and can be better industrialized; the obtained laminated aluminum alloy composite plate has excellent mechanical properties, and the interlayer bonding strength is greatly improved compared with the traditional process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation and processing of metal composite materials, and in particular to a laminated aluminum alloy composite plate and a preparation method thereof. Background Art

[0002] Armored vehicle protection materials are required to have the advantages of good processing performance, light weight, good impact resistance, excellent welding performance, and good corrosion resistance. At present, armored vehicle protection materials are mainly based on homogeneous armor, that is, armor with basically the same chemical composition, metallographic structure and mechanical properties in the cross section, but homogeneous armor is difficult to be effective against various anti-armor weapons at the same time. Although increasing the thickness of homogeneous armor can improve its protection ability, it will also increase the weight of the armored vehicle, resulting in a decrease in the flexibility of the vehicle. Therefore, in order to further improve the anti-ballistic performance of armored vehicles and protect against different anti-armor weapons at the same time, using materials with different properties to make composite armor materials has become the main direction of armor material development. The performance of composite armor is designable, that is, the structure and material can be designed within a certain range. A series of armors with different performances, different qualities and thicknesses can be designed according to the combat environment and the different parts of use, so as to meet various use requirements, including multi-layer aluminum alloy armor, titanium / aluminum multi-layer composite armor, steel / aluminum composite armor, etc. Although layered composite armor has a series of advantages, it has disadvantages such as complex manufacturing technology, high cost, and poor interlayer bonding. Therefore, providing a layered armor material with excellent comprehensive performance has become a problem to be solved urgently. Summary of the invention

[0003] The purpose of the present invention is to overcome the problems in the prior art and provide a laminated aluminum alloy composite plate and a preparation method thereof.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing a laminated aluminum alloy composite plate, comprising the following steps:

[0006] (1) performing homogenization treatment and surface treatment on the panel, the middle panel, and the back panel independently and sequentially to obtain a treated panel, a treated middle panel, and a treated back panel;

[0007] (2) stacking the processed front panel, the processed middle panel, and the processed back panel in order to obtain a composite panel;

[0008] (3) Preheating, rolling and online quenching the combined plate in sequence to obtain a composite plate;

[0009] (4) Performing aging treatment on the composite plate to obtain the laminated aluminum alloy composite plate.

[0010] Preferably, the material of the panel in step (1) is 7055 aluminum alloy, 7050 aluminum alloy or 7A62 aluminum alloy; the material of the middle plate is pure aluminum or 7A01 aluminum alloy; the material of the back plate is 7N01 aluminum alloy or 7A52 aluminum alloy.

[0011] Preferably, the heating temperature of the homogenization treatment in step (1) is 465-475° C., and the insulation time is 8-72 h.

[0012] Preferably, the surface treatment in step (1) is alkaline washing, water washing, acid washing and secondary water washing performed in sequence.

[0013] Preferably, the alkali washing solution is NaOH solution, the alkali washing time is 3 to 10 minutes, and the mass fraction of the NaOH solution is 5 to 15 wt%; the water washing temperature is 80 to 100 ° C, and the water washing time is 3 to 15 minutes; the acid washing solution is HNO 3 solution, the pickling time is 3 to 10 minutes, the HNO 3 The mass fraction of the solution is 5 to 15 wt %; the temperature of the secondary water washing is 5 to 15° C., and the time of the secondary water washing is 3 to 15 minutes.

[0014] Preferably, the temperature of the preheating treatment in step (3) is 450-490° C., and the time of the preheating treatment is 0.5-6 h.

[0015] Preferably, the rolling reduction rate in step (3) is greater than or equal to 40%, and the final rolling temperature is greater than or equal to 380°C; online quenching is performed during final rolling; the online quenching is performed by water quenching or air cooling, and the water quenching temperature is 10 to 30°C; the cooling rate of the air cooling is greater than or equal to 6°C / s.

[0016] Preferably, the temperature of the aging treatment in step (4) is 100 to 140° C., and the time of the aging treatment is 6 to 48 hours.

[0017] The invention also provides a laminated aluminum alloy composite plate obtained by the preparation method.

[0018] The beneficial effects of the present invention are:

[0019] 1. The present invention provides a short-process preparation method for laminated aluminum alloy composite plates with high interface bonding strength, wherein the panel, middle plate and back plate are homogenized; the panel, middle plate and back plate are surface treated; the treated plates are assembled into composite plates in the order of the panel, middle plate and back plate, and the front and rear ends are riveted together with rivets; the composite plates are rapidly subjected to large deformation composite rolling after high-temperature preheating treatment, and the composite plates are quenched online by strong air cooling or water quenching in the final rolling, and then subjected to aging treatment. High-temperature large deformation composite rolling improves the interface strength of the laminated aluminum alloy composite plate. The method is easy to operate, and large deformation rolling composite + online quenching eliminates the conventional artificial solid solution process, shortens the process flow, is highly efficient, and can be better industrialized.

[0020] 2. The present invention provides a laminated aluminum alloy composite plate having excellent mechanical properties and interlayer bonding strength, and the interlayer bonding strength is greatly improved compared with the traditional process. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the preparation process of laminated aluminum alloy composite plate;

[0022] Figure 2 This is a microstructure diagram of the back plate of the laminated aluminum alloy composite plate 1 in Example 1;

[0023] Figure 3 This is the microstructure diagram of the back plate of the laminated aluminum alloy composite plate 2 in comparative example 1. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing a laminated aluminum alloy composite plate, comprising the following steps:

[0025] (1) performing homogenization treatment and surface treatment on the panel, the middle panel, and the back panel independently and sequentially to obtain a treated panel, a treated middle panel, and a treated back panel;

[0026] (2) stacking the processed front panel, the processed middle panel, and the processed back panel in order to obtain a composite panel;

[0027] (3) Preheating, rolling and online quenching the combined plate in sequence to obtain a composite plate;

[0028] (4) Performing aging treatment on the composite plate to obtain the laminated aluminum alloy composite plate.

[0029] In the present invention, the material of the panel in step (1) is preferably 7055 aluminum alloy, 7050 aluminum alloy or 7A62 aluminum alloy; the material of the middle plate is preferably pure aluminum or 7A01 aluminum alloy; the material of the back plate is preferably 7N01 aluminum alloy or 7A52 aluminum alloy.

[0030] In the present invention, the heating temperature of the homogenization treatment in step (1) is preferably 465-475°C, more preferably 467-473°C, and more preferably 470°C; the holding time is preferably 8-72h, more preferably 18-62h, and more preferably 26-52h.

[0031] In the present invention, the surface treatment in step (1) is preferably carried out in sequence by alkali washing, water washing, acid washing and secondary water washing.

[0032] In the present invention, the alkali washing solution is preferably a NaOH solution; the alkali washing temperature is preferably 20-30°C, more preferably 22-28°C, and more preferably 24-26°C; the alkali washing time is preferably 3-10 min, more preferably 4-9 min, and more preferably 6-7 min; the mass fraction of the NaOH solution is preferably 5-15wt%, more preferably 7-13wt%, and more preferably 9-11wt%; the water washing temperature is preferably 80-100°C, more preferably 85-95°C, and more preferably 90°C; the water washing time is preferably 3-15 min, more preferably 5-13 min, and more preferably 7-11 min; the acid washing solution is preferably HNO 3 solution; the pickling temperature is preferably 20 to 30°C, more preferably 22 to 28°C, and more preferably 24 to 26°C; the pickling time is preferably 3 to 10 min, more preferably 4 to 9 min, and more preferably 6 to 7 min; the HNO 3 The mass fraction of the solution is preferably 5-15wt%, more preferably 7-13wt%, and more preferably 9-11wt%; the temperature of the secondary water washing is preferably 5-15°C, more preferably 7-13°C, and more preferably 9-11°C; the time of the secondary water washing is preferably 3-15min, more preferably 5-13min, and more preferably 7-11min.

[0033] In the present invention, after the surface treatment is completed, the treated front panel, the treated middle panel and the treated back panel are blown dry and subjected to interface grinding treatments independently and sequentially; the interface grinding treatment is preferably performed with a wire brush.

[0034] In the present invention, the stacking in step (2) comprises the following steps:

[0035] Holes are drilled at the front and rear ends of the processed panel, the processed middle plate and the processed back plate, and the processed panel, the processed middle plate and the processed back plate are stacked in order and riveted and fixed with aluminum alloy rivets to obtain a composite plate.

[0036] In the present invention, the temperature of the preheat treatment in step (3) is preferably 450-490°C, more preferably 460-480°C, and more preferably 470°C; the time of the preheat treatment is preferably 0.5-6h, more preferably 1-4h, and more preferably 2-3h.

[0037] In the present invention, the reduction ratio of the rolling in step (3) is preferably greater than or equal to 40%, further preferably greater than or equal to 45%, and more preferably greater than or equal to 50%; the final rolling temperature of the rolling is preferably greater than or equal to 380°C, further preferably greater than or equal to 385°C, and more preferably greater than or equal to 390°C.

[0038] In the present invention, the online quenching during the final rolling is specifically: the composite plate is immediately quenched online by utilizing the residual heat after the rolling is completed; the online quenching method is preferably water quenching or air cooling, and the temperature of the water quenching is preferably 10-30°C, more preferably 15-25°C, and more preferably 18-22°C; the cooling rate of the air cooling is preferably greater than or equal to 6°C / s, more preferably greater than or equal to 7°C / s, and more preferably greater than or equal to 8°C / s.

[0039] In the present invention, the temperature of the aging treatment in step (4) is preferably 100-140°C, more preferably 110-130°C, and more preferably 120°C; the time of the aging treatment is preferably 6-48h, more preferably 12-40h, and more preferably 20-30h.

[0040] The invention also provides a laminated aluminum alloy composite plate obtained by the preparation method.

[0041] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0042] Example 1

[0043] The 17 mm thick 7A62 aluminum alloy front plate, 1 mm thick pure aluminum alloy middle plate and 17 mm thick 7A52 aluminum alloy back plate were homogenized at 468 ° C for 36 h. The three plates were alkali washed at 25 ° C for 5 min using a 10 wt% NaOH solution, then rinsed with 80 ° C water for 7 min, and then washed with 10 wt% HNO 3The solution was pickled at 25°C for 5 minutes, and finally rinsed with 10°C water for 8 minutes, dried with hot air, and the interface was polished with a wire brush; holes were drilled at the front and rear ends of the treated panel, the treated middle plate, and the treated back plate, and the treated panel, the treated middle plate, and the treated back plate were stacked in order, and fixed with aluminum alloy rivets to obtain a composite plate; the composite plate was preheated at 470°C for 2 hours, and then quickly rolled after being taken out, the first pass was rolled from 35mm to 17mm, and the second pass was rolled from 17mm to 6mm, the final rolling temperature was 420°C, and quenched with 20°C water during the final rolling; then aging treatment was performed at 120°C for 24 hours to obtain a laminated aluminum alloy composite plate 1 with a thickness of 6mm. The specific preparation flow chart is as follows Figure 1 shown.

[0044] A comparative example 1 is set up, and the conditions of comparative example 1 are specifically as follows: other conditions are controlled unchanged, the composite plate is taken out after preheat treatment at 420°C for 2 hours, and the composite plate is rolled according to 35mm→25mm→18mm→12mm→6mm. After completion, the composite plate is solution treated at 470°C for 2 hours and water quenched at 20°C; then, an aging treatment is performed at 120°C for 24 hours to obtain a laminated aluminum alloy composite plate 2 with a thickness of 6 mm (that is, a plate obtained by a traditional process).

[0045] A comparative example 2 is set up, and the conditions of comparative example 2 are specifically as follows: other conditions are controlled unchanged, the composite plate is taken out after preheat treatment at 470°C for 2 hours, and the composite plate is rolled according to 35mm→25mm→18mm→12mm→6mm. After completion, the composite plate is solution treated at 470°C for 2 hours, and water quenched at 20°C; and then aged at 120°C for 24 hours to obtain a laminated aluminum alloy composite plate 3 with a thickness of 6 mm.

[0046] The 7A52 and 7A62 Vickers hardnesses of the laminated aluminum alloy composite plates 1, 2, and 3 were tested by a hardness tester, and the interlaminar shear strength of the laminated aluminum alloy was tested by a tensile shear test (the interlaminar shear strength reflects the interlaminar bonding strength of the plate). The results are shown in Table 1. The microstructure morphology of the back plates of the laminated aluminum alloy composite plates 1 and 2 in this embodiment was characterized, and the microstructure diagram of the back plate of the laminated aluminum alloy composite plate 1 was obtained, as shown in Table 1. Figure 2 As shown; the microstructure diagram of the back plate of the laminated aluminum alloy composite plate 2, as shown Figure 3 As shown in the table, it can be seen that the hardness of the laminated plate prepared by the present invention is higher than that of the 7A52 aluminum alloy prepared by the traditional process. This is mainly because the online quenching retains many long strips of deformation structure ( Figure 2 As shown), many recrystallized grains appeared in the sample 2 of the conventional process ( Figure 3 The interlaminar shear strength is increased by 22.1% and 30.6% compared with the laminated aluminum alloy composite plate 2 and the laminated aluminum alloy composite plate 3, respectively.

[0047] Table 1 Mechanical properties comparison table

[0048]

[0049] Example 2

[0050] The 7050 aluminum alloy front plate with a thickness of 20 mm, the 7A01 aluminum alloy middle plate with a thickness of 1 mm, and the 7N01 aluminum alloy back plate with a thickness of 15 mm were homogenized at 470 ° C for 60 h. The three plates were alkali-washed at 24 ° C for 6 min using a 13 wt% NaOH solution, and then rinsed with 90 ° C water for 9 min, and then washed with 13 wt% HNO 3 The solution was pickled at 27°C for 6 minutes, and finally rinsed with 13°C water for 6 minutes, dried with hot air, and the interface was polished with a wire brush; holes were drilled at the front and rear ends of the treated panel, the treated middle plate and the treated back plate, and the treated panel, the treated middle plate and the treated back plate were stacked in this order, and fixed with aluminum alloy rivets to obtain a composite plate; the composite plate was preheated at 460°C for 3 hours, and then quickly rolled after being taken out, the first pass was rolled from 36 mm to 17 mm, and the second pass was rolled from 17 mm to 6 mm. The temperature after rolling was 395°C, and the final rolling was quenched in water at 25°C; then an aging treatment was performed at 110°C for 32 hours to obtain a laminated aluminum alloy composite plate with a thickness of 6 mm.

[0051] A comparative example of the present embodiment is set up, and the conditions of the comparative example are specifically as follows: controlling other conditions unchanged, the composite plate is taken out after preheat treatment at 420°C for 2 hours, and the composite plate is rolled according to 36mm→25.5mm→18mm→12.5mm→6mm. After completion, the composite plate is solution treated at 470°C for 2 hours and water quenched at 25°C; and then aged at 110°C for 32 hours to obtain a laminated aluminum alloy composite plate with a thickness of 6 mm.

[0052] Using the same testing method as in Example 1, it was found that the interlaminar shear strength of the laminated aluminum alloy composite plate in this example was 96.5 MPa, and the interlaminar bonding strength was increased by 15.7% over that of the comparative example.

[0053] Example 3

[0054] The 7055 aluminum alloy front plate with a thickness of 18 mm, the 7A01 aluminum alloy middle plate with a thickness of 1.5 mm, and the 7N01 aluminum alloy back plate with a thickness of 16 mm were homogenized at 472 ° C for 27 h. The three plates were alkali-washed at 26 ° C for 8 min using a 7 wt % NaOH solution, and then rinsed with 100 ° C water for 5 min, and then washed with 7 wt % HNO 3The solution was pickled at 22°C for 8 minutes, and finally rinsed with 14°C water for 10 minutes, dried with hot air, and the interface was polished with a wire brush; holes were drilled at the front and rear ends of the treated panel, the treated middle plate and the treated back plate, and the treated panel, the treated middle plate and the treated back plate were stacked in this order, and fixed with aluminum alloy rivets to obtain a composite plate; the composite plate was preheated at 455°C for 4 hours, and then quickly rolled after being taken out, with the first pass rolling from 35.5 mm to 17 mm, and the second pass rolling from 17 mm to 6 mm. The temperature after rolling was 386°C, and the final rolling was quenched in water at 26°C; then an aging treatment was performed at 130°C for 12 hours to obtain a laminated aluminum alloy composite plate with a thickness of 5.8 mm.

[0055] A comparative example of the present embodiment is set up, and the conditions of the comparative example are specifically as follows: controlling other conditions unchanged, the composite plate is preheated at 420°C for 2 hours and then taken out, and the composite plate is rolled according to 35.5mm→24.5mm→18.5mm→11.5mm→5.8mm. After completion, the composite plate is solution treated at 470°C for 2 hours and water quenched at 26°C; and then aged at 130°C for 12 hours to obtain a laminated aluminum alloy composite plate with a thickness of 5.8 mm.

[0056] Using the same testing method as in Example 1, it was found that the interlaminar shear strength of the laminated aluminum alloy composite plate in this example was 98.2 MPa, and the interlaminar bonding strength was increased by 17.2% over that of the comparative example.

[0057] It can be seen from the above embodiments that the present invention provides a method for preparing a laminated aluminum alloy composite plate, which utilizes the good plasticity of metal under high temperature conditions and adopts high temperature and large rolling deformation to improve the interface strength of the composite plate; the online quenching process is used to replace the traditional offline artificial solution process, shortening the process flow and improving the processing efficiency; it has the characteristics of simple preparation technology and easy engineering implementation. The prepared laminated aluminum alloy composite plate has excellent mechanical properties and interlaminar shear strength, and the interlaminar shear bonding strength is greatly improved.

[0058] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a laminated aluminum alloy composite plate, characterized in that: It includes the following steps: (1) performing homogenization treatment and surface treatment on the panel, the middle panel, and the back panel independently and sequentially to obtain a treated panel, a treated middle panel, and a treated back panel; The material of the panel in step (1) is 7055 aluminum alloy, 7050 aluminum alloy or 7A62 aluminum alloy; the material of the middle plate is pure aluminum or 7A01 aluminum alloy; the material of the back plate is 7N01 aluminum alloy or 7A52 aluminum alloy; The heating temperature of the homogenization treatment in step (1) is 465-475° C., and the holding time is 8-72 hours; (2) stacking the processed front panel, the processed middle panel and the processed back panel in order to obtain a composite panel; (3) Preheating, rolling and online quenching the combined plate in sequence to obtain a composite plate; In step (3), the rolling reduction ratio is greater than or equal to 40%, and the final rolling temperature is 380-420° C.; online quenching is performed during the final rolling; the online quenching method is water quenching or air cooling, and the water quenching temperature is 10-30° C.; the cooling rate of the air cooling is greater than or equal to 6° C. / s; (4) performing aging treatment on the composite plate to obtain the laminated aluminum alloy composite plate; The temperature of the aging treatment in step (4) is 100 to 140° C., and the time of the aging treatment is 12 to 48 hours.

2. The preparation method according to claim 1, characterized in that The surface treatment in step (1) is alkali washing, water washing, acid washing and secondary water washing performed in sequence.

3. The preparation method according to claim 2, characterized in that: The alkali washing solution is a NaOH solution, the alkali washing time is 3 to 10 minutes, and the mass fraction of the NaOH solution is 5 to 15wt%; the water washing temperature is 80 to 100°C, and the water washing time is 3 to 15 minutes; the acid washing solution is an HNO3 solution, the acid washing time is 3 to 10 minutes, and the mass fraction of the HNO3 solution is 5 to 15wt%; the secondary water washing temperature is 5 to 15°C, and the secondary water washing time is 3 to 15 minutes.

4. The preparation method according to claim 1, characterized in that: The temperature of the preheating treatment in step (3) is 450-490° C., and the time of the preheating treatment is 0.5-6 hours.

5. The laminated aluminum alloy composite plate obtained by the preparation method according to any one of claims 1 to 4.