Ionic polyurethane composition and preparation method and application thereof

By introducing ionic groups into the polyurethane composition, using chemical grafting and physical mixing technology, the problems of the decrease in strength and elasticity of the polyurethane elastomer in a high temperature environment are solved, and high toughness, high strength and excellent fatigue resistance are achieved. Ionic polyurethane composition suitable for high-performance bicycle tires.

CN115677970BActive Publication Date: 2024-11-12WANHUA CHEM BEIJING
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211433842.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-11-12
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

The strength of existing polyurethane elastomers decreases in high temperature environments, and increasing the hard segment content or using polyester-type raw materials with higher strength will lead to a decrease in elasticity and toughness, making it difficult to take into account high toughness, high strength and excellent fatigue resistance.

Method used

Ion polyurethane composition is prepared by chemical grafting and physical mixing.

Benefits of technology

The strength, fatigue resistance and thermal stability of polyurethane elastomer have been significantly improved, making it suitable for the preparation of high-performance single-vehicle tires. The fatigue test shows that the number of obstacle blocks has been exceeded 3 million to 3.2 million times, and the rebound rate is 60 to 65%. The initial decomposition temperature is 221-260℃, the tensile strength is 4.3-5.2MPa, the elongation rate of break is 177-230%, and the wear is 1.9-2.1%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003946101110000051
    Figure BDA0003946101110000051
  • Figure BDA0003946101110000091
    Figure BDA0003946101110000091
  • Figure BDA0003946101110000161
    Figure BDA0003946101110000161
Patent Text Reader

Abstract

The invention provides an ionic polyurethane composition and a preparation method and application thereof. The ionic polyurethane composition comprises an ionic prepolymer and an ionic composition. The raw materials for preparing the ionic prepolymer comprise polyether polyol A, polyisocyanate and a compound containing ionic groups terminated by active groups. The ionic composition comprises an aqueous solution containing ionic groups, polyether polyol B, a chain extender and a catalyst. The invention introduces ionic groups into polyurethane molecular chains by chemical grafting and physical mixing, thereby enhancing the interaction force between polyurethane molecules, thereby effectively improving the mechanical properties, fatigue resistance and thermal stability of a polyurethane elastomer prepared by using the ionic polyurethane composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane resins, and in particular relates to an ionic polyurethane composition and a preparation method and application thereof. Background Art

[0002] Polyurethane elastomer is a special category of elastomers. Its main macromolecular chain is composed of flexible segments (also called soft segments) with a glass transition temperature below room temperature and rigid segments (also called hard segments) with a glass transition temperature above room temperature. The electrostatic force between the hard segments is very strong, and a large number of hydrogen bonds are often generated. This strong electrostatic force, in addition to directly affecting the mechanical properties, can also promote the aggregation of hard segments, produce microphase separation, and improve the mechanical properties and high and low temperature properties of the elastomer. The raw materials of polyurethane elastomers are of various types, the formulas are diverse, and the adjustable range is very large. The hardness range of the obtained polyurethane elastomer is very wide, ranging from low modulus rubber below A10 to high impact elastomer of D90, which greatly exceeds the elastic modulus of other rubbers. Therefore, the performance range of polyurethane elastomer is very wide. The lower limit of its hardness and elastic modulus range exceeds rubber, and the upper limit almost covers plastics. It has a wide range of applications in people's lives.

[0003] However, due to the large number of polar groups in the molecular structure of polyurethane elastomers, the intramolecular force and intermolecular force are large, and there may be other factors that hinder the free rotation of single bonds, the stress and strain of the polyurethane elastomer cannot reach equilibrium instantaneously, and it exhibits hysteresis under the action of alternating stress, causing endogenous heat, which seriously affects the performance of the product. As a result, the strength of the polyurethane elastomer decreases significantly in a high temperature environment. At 70-80°C, its tear strength decreases to about half of that at room temperature, and the tensile strength and wear resistance also show similar patterns.

[0004] At present, increasing the hard segment content of polyurethane or using polyester raw materials with higher strength are common means to improve the above problems. CN113980232A discloses a thermoplastic polyurethane elastomer that takes into account both ultra-low temperature resistance and high mechanical properties and its preparation method. The soft segment of the thermoplastic polyurethane elastomer described in the invention is composed of polytetramethylene ether diol, and the hard segment is composed of 4,4'-dicyclohexylmethane diisocyanate and a new type of small molecule diamine cyclic chain extender. The thermoplastic polyurethane elastomer that takes into account ultra-low temperature resistance and high mechanical properties is prepared by solution polymerization and a two-step method. Its synthesis method is simple, and the glass transition temperature can be as low as -104°C, which is suitable for extremely cold environments. At the same time, it also takes into account the mechanical properties of the thermoplastic polyurethane elastomer, and the tensile strength is as high as 47MPa.

[0005] However, although the strength and fatigue resistance of the tire can be improved by increasing the hard segment content of the polyurethane or using higher-strength polyester raw materials, the elasticity and toughness of the polyurethane elastomer will decrease, seriously affecting its application.

[0006] Therefore, developing an ionic polyurethane composition having high toughness, high strength and excellent fatigue resistance is a technical problem that needs to be solved urgently in the art. Summary of the invention

[0007] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an ionic polyurethane composition and a preparation method and application thereof. The ionic polyurethane composition introduces ionic groups into the preparation raw materials by chemical grafting and physical mixing, which effectively enhances the interaction force between polyurethane elastomer molecules, thereby effectively improving the strength and fatigue resistance of the polyurethane elastomer prepared by using the ionic polyurethane composition without affecting its toughness, making it suitable for preparing bicycle tires.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides an ionic polyurethane composition, the ionic polyurethane composition comprising an ionic prepolymer and an ionic composition;

[0010] The raw materials for preparing the ionic prepolymer include polyether polyol A, polyisocyanate and a compound containing an ionic group terminated with an active group;

[0011] The ionic composition comprises polyether polyol B, an aqueous solution containing ionic groups, a chain extender and a catalyst.

[0012] The ionic polyurethane composition provided by the present invention comprises an ionic prepolymer and an ionic composition. On the one hand, the ionic prepolymer is prepared by selecting an active group-terminated ionic group-containing compound, collocating polyether polyol A and polyisocyanate, and the ionic group is introduced into the polyurethane molecular chain by chemical grafting. On the other hand, the ionic group-containing aqueous solution is selected and collocated with polyether polyol B to form the ionic composition, and the ionic group is introduced into the polyurethane molecular chain by physical mixing. The physical mixing and chemical grafting are combined to greatly increase the content of the ionic group in the polymer. On the one hand, when chemical grafting is used alone, the addition amount is limited due to the problem of violent reaction between small molecules and isocyanate. On the other hand, when physical mixing is used alone, the amount of water used in the system cannot be too much, so the amount of the ionic group aqueous solution cannot be too much.

[0013] Specifically, ionic groups are introduced into the polyurethane molecular chain and its polyurethane system, and the strong polarity of the ionic groups is utilized to form hydrogen bonds with groups such as carbamate in the polyurethane, and the physical cross-linking bonds can be formed by utilizing the dipole-dipole interaction between the ionic groups, thereby effectively enhancing the interaction between the polyurethane molecules, thereby improving the mechanical properties, toughness, thermal stability and fatigue resistance of the ionic polyurethane elastomer prepared by using the ionic polyurethane composition.

[0014] Preferably, the mass ratio of the ionic prepolymer to the ionic composition is (0.7-1.3):1, for example, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1, 1:1, 1.1:1 or 1.2:1, etc.

[0015] Preferably, the reactive group-terminated ionic group-containing compound comprises a hydroxyl-terminated ionic group-containing compound and / or an amino-terminated ionic group-containing compound.

[0016] Preferably, the active group-terminated ionic group-containing compound includes any one of 2-sodium sulfonate-1,4-butanediol, sodium diaminocarboxylate, sodium ethylenediamine ethanesulfonate, dihydroxymethylpropionic acid, tris(2-hydroxyethyl)methyl sulfate, zinc citrate, monosodium citrate or disodium citrate, or a combination of at least two thereof.

[0017] Preferably, the polyether polyol A and the polyether polyol B each independently include any one of polymer polyol, polypropylene glycol or polytetramethylene glycol, or a combination of at least two thereof.

[0018] It should be noted that the "polymer polyols" mentioned in the present invention specifically refer to vinyl polymer grafted polyether polyols, referred to as POP.

[0019] Preferably, the number average molecular weight of the polyether polyol A and the polyether polyol B is independently 1000-6000, for example, 1300, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000 or 5500.

[0020] Preferably, the functionality of the polyether polyol A and the polyether polyol B is independently 2-3.

[0021] Preferably, the number average molecular weight of the polytetrahydrofuran diol is 1000-3000, for example 1200, 1400, 1600, 1800, 2000, 2200, 2400, 2600 or 2800 etc.

[0022] Preferably, the polyisocyanate includes any one of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI) or carbodiimide-modified MDI, or a combination of at least two thereof.

[0023] Preferably, the raw materials for preparing the ionic prepolymer include the following components in parts by weight:

[0024] Polyether polyol A 30-50 parts by weight

[0025] Polyisocyanate 47-69 parts by weight

[0026] 1 to 3 parts by weight of the active group-terminated ionic group-containing compound.

[0027] Wherein, the polyether polyol A may be 32 parts by weight, 34 parts by weight, 36 parts by weight, 38 parts by weight, 40 parts by weight, 42 parts by weight, 44 parts by weight, 46 parts by weight or 48 parts by weight, etc.

[0028] The polyisocyanate may be 50 parts by weight, 53 parts by weight, 56 parts by weight, 59 parts by weight, 63 parts by weight, 65 parts by weight, 67 parts by weight, etc.

[0029] The active group-terminated ionic group-containing compound may be 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, 1.8 parts by weight, 2 parts by weight, 2.2 parts by weight, 2.4 parts by weight, 2.6 parts by weight, 2.8 parts by weight, etc.

[0030] Preferably, the aqueous solution containing ionic groups includes any one of an aqueous solution of monosodium citrate, an aqueous solution of disodium citrate or an aqueous solution of zinc citrate, or a combination of at least two of them.

[0031] Preferably, the mass ratio of solute to water in the aqueous solution containing ionic groups is 1:(2-4), for example, 1:2.2, 1:2.4, 1:2.6, 1:2.8, 1:3, 1:3.2, 1:3.4, 1:3.6 or 1:3.8, etc.

[0032] Preferably, the chain extender includes any one of ethylene glycol, butanediol, diethylene glycol, triethylene glycol, dipropylene glycol, diethylene glycol, neopentyl glycol, glycerol, trimethylolpropane, pentaerythritol or sorbitol, or a combination of at least two thereof.

[0033] Preferably, the catalyst comprises an organotin catalyst.

[0034] Preferably, the ionic composition comprises the following components in parts by weight:

[0035]

[0036] The aqueous solution containing ionic groups may be 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight or 0.45 parts by weight.

[0037] The polyether polyol B may be 82 parts by weight, 84 parts by weight, 86 parts by weight, 88 parts by weight, etc.

[0038] The chain extender can be 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight or 14 parts by weight, etc.

[0039] The catalyst may be 0.02 parts by weight, 0.04 parts by weight, 0.06 parts by weight, 0.08 parts by weight, 0.1 parts by weight, 0.12 parts by weight, 0.14 parts by weight, 0.16 parts by weight, 0.18 parts by weight, etc.

[0040] Preferably, the ionic composition further comprises silicone oil and / or color paste.

[0041] Preferably, the content of silicone oil in the ionic composition is 1 to 2 parts by weight, for example, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight or 1.9 parts by weight.

[0042] Preferably, the content of the color paste in the ionic composition is 2 to 4 parts by weight, for example, 2.2 parts by weight, 2.4 parts by weight, 2.6 parts by weight, 2.8 parts by weight, 3 parts by weight, 3.2 parts by weight, 3.4 parts by weight, 3.6 parts by weight or 3.8 parts by weight.

[0043] In a second aspect, the present invention provides a method for preparing the ionic polyurethane composition as described in the first aspect, the preparation method comprising preparing an ionic prepolymer and preparing an ionic composition;

[0044] The preparation method of the ionic prepolymer comprises: reacting polyether polyol A and part of polyisocyanate, adding a compound containing an ionic group terminated with an active group to react, and then adding the remaining part of polyisocyanate to mix, thereby obtaining the ionic prepolymer;

[0045] The preparation method of the ionic composition comprises: mixing polyether polyol B, an aqueous solution containing ionic groups, a chain extender, a catalyst, optionally silicone oil and optionally color paste to obtain the ionic composition.

[0046] Preferably, the reaction time of the polyether polyol A and part of the polyisocyanate is 3 to 6 hours, for example, 3.5 hours, 4 hours, 4.5 hours, 5 hours or 5.5 hours.

[0047] Preferably, the reaction temperature of the polyether polyol A and part of the polyisocyanate is 60-100°C, for example, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C.

[0048] Preferably, the reaction time of adding the active group-capped ionic group-containing compound is 2 to 4 h, for example, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h or 3.8 h.

[0049] Preferably, the reaction temperature for reacting the compound containing ionic groups capped with active groups is 60-100°C, for example, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C.

[0050] Preferably, the adding of the remaining part of the polyisocyanate for mixing is carried out at a temperature below 60° C. (eg, 55° C., 50° C., 45° C., 40° C., 35° C. or 30° C., etc.).

[0051] Preferably, the mixing time for adding the remaining part of the polyisocyanate is 5 to 20 minutes, for example, 7 minutes, 8 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, 18 minutes or 19 minutes.

[0052] Preferably, the mixing time of the polyether polyol B, the aqueous solution containing ionic groups, the chain extender, the catalyst, the optional silicone oil and the optional color paste is 0.5 to 1 h, such as 0.6 h, 0.7 h, 0.8 h or 0.9 h.

[0053] In a third aspect, the present invention provides an ionic polyurethane elastomer, wherein the raw materials for preparing the ionic polyurethane elastomer include the ionic polyurethane composition as described in the first aspect.

[0054] In a fourth aspect, the present invention provides a method for preparing the ionic polyurethane elastomer as described in the third aspect, the preparation method comprising: mixing the ionic prepolymer and the ionic composition in the ionic polyurethane elastomer as described in the first aspect, curing and foaming, to obtain the ionic polyurethane elastomer.

[0055] In a fifth aspect, the present invention provides an ionic polyurethane tire, wherein the raw materials for preparing the ionic polyurethane tire include the ionic polyurethane composition as described in the first aspect.

[0056] Preferably, the ionic polyurethane tire is an ionic polyurethane bicycle tire.

[0057] Preferably, the density of the ionic polyurethane tire is 500-600 kg / m 3 , for example 510kg / m 3 , 520kg / m 3 , 530kg / m 3 、540kg / m 3 、550kg / m 3 、560kg / m 3 、570kg / m 3 、580kg / m 3 or 590kg / m 3 wait.

[0058] In a sixth aspect, the present invention provides a method for preparing the ionic polyurethane tire as described in the fifth aspect, the preparation method comprising: mixing the ionic prepolymer and the ionic composition in the ionic polyurethane elastomer as described in the first aspect, pouring them into a mold, curing and foaming, and obtaining the ionic polyurethane tire.

[0059] Preferably, the mass ratio of the ionic prepolymer to the ionic composition is (0.7-1.3):1, for example, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1, 1:1, 1.1:1 or 1.2:1, etc.

[0060] Preferably, the temperature of the mold is 45-65°C, for example, 47°C, 49°C, 50°C, 51°C, 52°C, 53°C or 54°C.

[0061] Preferably, the rotation speed of the mold is 500-800 m / min, for example, 550 m / min, 600 m / min, 650 m / min, 700 m / min or 750 m / min.

[0062] Preferably, the step of opening the mold is further included after the curing and foaming.

[0063] Preferably, the mold opening time is 3 to 10 minutes, for example, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes or 9 minutes.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] (1) The ionic polyurethane composition provided by the present invention comprises an ionic prepolymer and an ionic composition, wherein the raw materials for preparing the ionic prepolymer comprise polyether polyol A, polyisocyanate and an ionic group-containing compound terminated with an active group, and the ionic composition comprises an ionic group-containing aqueous solution, polyether polyol B, a chain extender and a catalyst; the ionic groups are introduced into the polyurethane molecular chain by chemical grafting and physical mixing, thereby enhancing the interaction force between polyurethane molecules, thereby effectively improving the mechanical properties, fatigue resistance and thermal stability of the polyurethane elastomer prepared by using the ionic polyurethane composition.

[0066] (2) Specifically, by further limiting the amount of the compound containing ionic groups capped with active groups in the ionic prepolymer and limiting the content of ionic groups in the ionic composition, the fatigue test of the finally obtained polyurethane tire can show that the number of times of passing the obstacle block is as high as 3 million to 3.2 million times, the rebound rate is 60 to 65%, the initial decomposition temperature is 221 to 260°C, the tensile strength is 4.3 to 5.2 MPa, the elongation at break is 177 to 230%, and the abrasion is 1.9 to 2.1%. DETAILED DESCRIPTION

[0067] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0068] The detailed information of the raw materials involved in the specific implementation method is shown in Table 1:

[0069] Table 1

[0070]

[0071] Example 1

[0072] An ionic polyurethane composition, comprising an ionic polyurethane elastomer including an ionic prepolymer and an ionic composition in a mass ratio of 0.94:1;

[0073] The preparation method of the ionic prepolymer comprises: adding 60g of diphenylmethane diisocyanate and 34g of polytetrahydrofuran polyol to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen gas device, reacting at 80°C for 4h, then adding 2.5g of sodium ethylenediamine sulfonate and continuing to react at 80°C for 2h, naturally cooling to 55°C, then adding 5g of carbodiimide-modified MDI and stirring for 5min, filtering solid impurities, and obtaining the ionic prepolymer;

[0074] The ionic composition and preparation method include: mixing 100g of polytetrahydrofuran polyol, 0.3g of an ionic group-containing aqueous solution (composed of monosodium citrate and water in a mass ratio of 1:3), 10g of ethylene glycol, 0.05g of an organic tin catalyst, 1g of dimethyl silicone oil and 2g of a color paste for 1 hour to obtain the ionic composition.

[0075] Example 2

[0076] An ionic polyurethane composition, comprising an ionic polyurethane elastomer including an ionic prepolymer and an ionic composition in a mass ratio of 0.88:1;

[0077] The preparation method of the ionic prepolymer comprises: adding 60g of diphenylmethane diisocyanate and 38.5g of polypropylene glycol A to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen gas device, reacting at 90°C for 3.5h, then adding 1g of sodium ethylenediamine sulfonate and continuing to react at 90°C for 2h, naturally cooling to 55°C, then adding 3g of carbodiimide-modified MDI and stirring for 5min, filtering solid impurities, and obtaining the ionic prepolymer;

[0078] The preparation method of the ionic composition comprises: mixing 100g of polypropylene glycol A, 0.28g of an aqueous solution containing ionic groups (composed of disodium citrate and water in a mass ratio of 1:4), 14g of butanediol, 0.05g of an organic tin catalyst, 1g of dimethyl silicone oil and 2g of a color paste for 1 hour to obtain the ionic composition.

[0079] Example 3

[0080] An ionic polyurethane composition, comprising an ionic polyurethane elastomer including an ionic prepolymer and an ionic composition in a mass ratio of 0.93:1;

[0081] The preparation method of the ionic prepolymer includes: adding 57.5g of diphenylmethane diisocyanate, 5g of isophorone diisocyanate and 35g of polypropylene glycol B to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen gas device, reacting at 75°C for 5h, then adding 1.5g of 2-sodium sulfonate-1,4-butanediol and continuing to react at 75°C for 3h, naturally cooling to 55°C, then adding 3g of carbodiimide-modified MDI and stirring for 5min, filtering solid impurities, and obtaining the ionic prepolymer;

[0082] The ionic composition and preparation method include: mixing 100g of polytetrahydrofuran polyol, 0.27g of an ionic group-containing aqueous solution (composed of zinc citrate and water in a mass ratio of 1:4), 8g of butanediol, 6g of propylene glycol, 0.05g of an organic tin catalyst, 1g of dimethyl silicone oil and 2g of a color paste for 1 hour to obtain the ionic composition.

[0083] Example 4

[0084] An ionic polyurethane composition, comprising an ionic polyurethane elastomer including an ionic prepolymer and an ionic composition in a mass ratio of 0.94:1;

[0085] The preparation method of the ionic prepolymer comprises: adding 55.5g of diphenylmethane diisocyanate, 5g of isophorone diisocyanate and 34g of polytetrahydrofuran polyol to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen gas device, reacting at 75°C for 5h, then adding 2.5g of sodium diaminocarboxylate and continuing to react at 95°C for 2h, naturally cooling to 55°C, then adding 4g of carbodiimide-modified MDI and stirring for 5min, filtering solid impurities, and obtaining the ionic prepolymer;

[0086] The ionic composition and preparation method include: mixing 80g of polytetrahydrofuran polyol, 10g of polymer polyol, 0.32g of an ionic group-containing aqueous solution (composed of monosodium citrate, zinc citrate and water in a mass ratio of 0.5:0.5:3), 10g of a chain extender (composed of ethylene glycol and glycerol in a mass ratio of 19:1), 0.05g of an organic tin catalyst, 1g of dimethyl silicone oil and 2g of a color paste for 1 hour to obtain the ionic composition.

[0087] Example 5

[0088] An ionic polyurethane composition, which differs from Example 1 only in that the amount of sodium ethylenediamine sulfonate added to the ionic prepolymer is 3g, the amount of diphenylmethane diisocyanate used is 62g, and the amount of polytetrahydrofuran polyol used is 33.5g, and other components, amounts and preparation methods are the same as those in Example 1.

[0089] Example 6

[0090] An ionic polyurethane composition, which differs from Example 1 only in that the addition amount of sodium ethylenediamine sulfonate in the ionic prepolymer is 1g, the amount of diphenylmethane diisocyanate is 58g, and the amount of polytetrahydrofuran polyol is 38g, and other components, amounts and preparation methods are the same as those in Example 1.

[0091] Example 7

[0092] An ionic polyurethane composition, which differs from Example 1 only in that the addition amount of sodium ethylenediamine sulfonate in the ionic prepolymer is 0.5g, the amount of diphenylmethane diisocyanate is 57g, and the amount of polytetrahydrofuran polyol is 39g; other components, amounts and preparation methods are the same as those in Example 1.

[0093] Example 8

[0094] An ionic polyurethane composition, which differs from Example 1 only in that the amount of sodium ethylenediamine sulfonate added to the ionic prepolymer is 4g, the amount of diphenylmethane diisocyanate used is 69g, and the amount of polytetrahydrofuran polyol used is 34.5g; other components, amounts and preparation methods are the same as those in Example 1.

[0095] Example 9

[0096] An ionic polyurethane elastomer is different from Example 1 only in that the amount of the aqueous solution containing ionic groups in the ionic composition is 0.1 g, and 0.2 g of water is additionally added, and the other components, amounts and preparation methods are the same as those in Example 1.

[0097] Example 10

[0098] An ionic polyurethane composition is different from Example 1 only in that the amount of the aqueous solution containing ionic groups added to the ionic composition is 0.4 g, and the other components, amounts and preparation methods are the same as those in Example 1.

[0099] Embodiment 11

[0100] An ionic polyurethane composition is different from Example 1 only in that the amount of the aqueous solution containing ionic groups in the ionic composition is 0.05 g, and 0.25 g of water is additionally added; the other components, amounts and preparation methods are the same as those in Example 1.

[0101] Example 12

[0102] An ionic polyurethane composition is different from Example 1 only in that the amount of the aqueous solution containing ionic groups added to the ionic composition is 0.5 g, and the other components, amounts and preparation methods are the same as those in Example 1.

[0103] Comparative Example 1

[0104] An ionic polyurethane composition, which differs from Example 1 in that the mass ratio of the ionic prepolymer to the ionic composition is 0.83:1, and no aqueous solution containing ionic groups is added to the ionic composition, and 0.23 g of water is additionally added; sodium ethylenediamine sulfonate is not added to the ionic prepolymer, and other components, amounts and preparation methods are the same as those in Example 1.

[0105] Comparative Example 2

[0106] An ionic polyurethane composition, which differs from Example 1 in that the mass ratio of the ionic prepolymer to the ionic composition is 0.84:1, and sodium ethylenediamine sulfonate is not added to the ionic prepolymer, and other components, amounts and preparation methods are the same as those in Example 1.

[0107] Comparative Example 3

[0108] An ionic polyurethane composition, which differs from Example 1 in that the mass ratio of the ionic prepolymer to the ionic composition is 0.93:1, and no aqueous solution containing ionic groups is added to the ionic composition, and 0.23 g of water is additionally added, and other components, amounts and preparation methods are the same as those in Example 1.

[0109] Application Example 1

[0110] An ionic polyurethane tire, the preparation method of which comprises: mixing the ionic prepolymer (40° C.) and the ionic composition (40° C.) in the ionic polyurethane composition provided in Example 1 in a total amount of 1000 g at a mass ratio of 0.95:1 by a low-pressure foaming machine, pouring into a tire mold at 60° C. and a rotation speed of 800 m / min, curing and foaming for 4 minutes, opening the mold, and obtaining a tire with a density of 600 kg / m 3 Ionic polyurethane tires.

[0111] Application Example 2

[0112] An ionic polyurethane tire, the preparation method of which comprises: mixing the ionic prepolymer (40° C.) and the ionic composition (45° C.) in the ionic polyurethane composition provided in Example 2 with a total amount of 1000 g at a mass ratio of 0.92:1 by a low-pressure foaming machine, pouring into a tire mold at 60° C. and a rotation speed of 700 m / min, curing and foaming for 5 minutes, opening the mold, and obtaining a tire with a density of 600 kg / m 3 Ionic polyurethane tires.

[0113] Application Example 3

[0114] An ionic polyurethane tire, the preparation method of which comprises: mixing the ionic prepolymer (45° C.) and the ionic composition (40° C.) in the ionic polyurethane composition provided in Example 3 with a total amount of 1000 g at a mass ratio of 0.90:1 by a low-pressure foaming machine, pouring into a tire mold at 55° C. and a rotation speed of 600 m / min, curing and foaming for 5 minutes, opening the mold, and obtaining a tire with a density of 600 kg / m 3 Ionic polyurethane tires.

[0115] Application Example 4

[0116] An ionic polyurethane tire, the preparation method of which comprises: mixing the ionic prepolymer (40°C) and the ionic composition (40°C) in the ionic polyurethane composition provided in Example 4 with a total amount of 1000g at a mass ratio of 0.88:1 by a low-pressure foaming machine, pouring into a tire mold at 60°C and a rotation speed of 560r / min, curing and foaming for 4min, opening the mold, and obtaining a tire with a density of 600kg / m 3Ionic polyurethane tires.

[0117] Application Examples 5 to 12

[0118] An ionic polyurethane tire, which differs from Application Example 1 only in that the ionic polyurethane compositions obtained in Examples 5 to 12 are used to replace the ionic polyurethane composition obtained in Example 1, and other steps and parameters are the same as those in Application Example 1.

[0119] Comparative Application Examples 1 to 3

[0120] An ionic polyurethane tire, which differs from Application Example 1 only in that the ionic polyurethane compositions obtained in Comparative Examples 1 to 3 are used to replace the ionic polyurethane composition obtained in Example 1, and other steps and parameters are the same as those in Application Example 1.

[0121] Performance Test:

[0122] (1) Fatigue resistance: The test is carried out in accordance with the test method provided in "Bicycle Safety Requirements ISO-4210"; the specific test requirements are as follows: radial load 640N, hitting the obstacle at a speed of 25KM / H (±10%), roller diameter 500-1000mm, obstacle block width 50±2.5mm, thickness 10±0.25mm, 45 degrees chamfer at half thickness, adjacent obstacle blocks are not less than 400mm, before the tire is damaged, the more times it hits the obstacle bar, the better the fatigue resistance.

[0123] (2) Wear: The tires were subjected to wear tests in accordance with GB9867. The specific test methods were as follows: specimen load 5±0.2N; fixture lateral displacement 4.2±0.04mm / roller turn; roller diameter 150±2mm; roller length 460mm; roller speed 40±2rpm; wear stroke 40m equivalent to 84 turns; wear speed 0.32m / sec; inclination 3°; cylindrical specimen specifications: diameter 16±2mm, height <6mm; balance measurement accuracy required for wear data reading is ±1mg;

[0124] (3) Rebound performance: The rebound test is carried out in accordance with ASTM D2632. The drop height of the hammer is 400 mm; the mass of the hammer is 28 g ± 0.5 g; the impact kinetic energy is 0.11 J; the diameter of the product slice is required to be no less than 32 mm, the thickness of the product slice is 11 ± 1 mm, and the cut surface is required to be flat; the experiment is divided into 2 groups (5 test pieces in each group), and the test temperature is 23 ° C. Tests are carried out according to the above conditions and the results are recorded;

[0125] (4) Tensile strength and elongation at break: tested in accordance with the test method provided in GB / T2568-1995;

[0126] (5) Initial decomposition temperature: The TG curve of the polyurethane tire is detected by a thermogravimetric analyzer to characterize its heat resistance. The test sample weight is 5-10 mg, and the N2 flow rate is 10 mL min -1 , heating rate is 10℃·min -1 , the test temperature range is 25~400℃.

[0127] According to the above test method, the ionic polyurethane tires provided in Examples 1 to 12 and Comparative Application Examples 1 to 3 were tested, and the test results are shown in Table 2:

[0128] Table 2

[0129]

[0130] According to the data in Table 2, it can be seen that the ionic polyurethane tire made from the ionic polyurethane composition provided by the present invention has excellent mechanical properties, fatigue resistance and thermal stability; and by further limiting the content of the ionic groups therein, the fatigue test of the finally obtained polyurethane tire can show that the number of times of passing through the obstacle block is as high as 3 million to 3.2 million times, the rebound performance is 60 to 65%, the initial decomposition temperature is 221 to 260° C., the tensile strength is 4.3 to 5.2 MPa, the elongation at break is 177 to 230%, and the abrasion is 1.9 to 2.1%. By comparing the data of Application Example 1 and Comparative Examples 1 to 3, it can be seen that the number of times the ionic polyurethane tires pass through the obstacle block, the elasticity and the initial decomposition temperature are lower when no ionic groups are added to the ionic composition, no sodium ethylenediamine ethanesulfonate is added to the ionic prepolymer (Comparative Application Example 1), no sodium ethylenediamine ethanesulfonate is added to the ionic prepolymer (Comparative Application Example 2), and no ionic groups are added to the ionic composition (Comparative Application Example 3), indicating that the fatigue performance and heat resistance of the polyurethane tires obtained in Comparative Application Examples 1 to 3 are poor.

[0131] Further comparing the data of Application Example 1 with Application Examples 5 to 8, and comparing the data of Application Example 1 with Application Examples 9 to 12, it can be found that if the amount of ionic groups added to the ionic composition is not within the range defined by the present invention, or the amount of the active group-terminated ionic group-containing compound added to the ionic prepolymer is not within the range defined by the present invention, the fatigue performance and thermal stability of the final polyurethane tire will be reduced.

[0132] The applicant declares that the present invention illustrates the ionic polyurethane composition and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An ionic polyurethane composition, characterized in that: The ionic polyurethane composition comprises an ionic prepolymer and an ionic composition; The raw materials for preparing the ionic prepolymer include the following components in parts by weight: Polyether polyol A 30-50 parts by weight Polyisocyanate 47-69 parts by weight 1 to 3 parts by weight of a compound containing an ionic group capped with an active group; The active group-terminated ionic group-containing compound includes a hydroxyl-terminated ionic group-containing compound and / or an amino-terminated ionic group-containing compound; The polyisocyanate includes any one of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate or carbodiimide-modified MDI or a combination of at least two thereof; The ionic composition comprises the following components in parts by weight: The aqueous solution containing ionic groups includes any one of an aqueous solution of monosodium citrate, an aqueous solution of disodium citrate or an aqueous solution of zinc citrate, or a combination of at least two thereof; The chain extender includes any one of ethylene glycol, butanediol, diethylene glycol, triethylene glycol, dipropylene glycol, diethylene glycol, neopentyl glycol, glycerol, trimethylolpropane, pentaerythritol or sorbitol, or a combination of at least two thereof.

2. The ionic polyurethane composition according to claim 1, characterized in that The mass ratio of the ionic prepolymer to the ionic composition is (0.7-1.3):

1.

3. The ionic polyurethane composition according to claim 1, characterized in that The active group-terminated ionic group-containing compound includes any one of 2-sodium sulfonate-1,4-butanediol, sodium diaminocarboxylate, sodium ethylenediamine ethanesulfonate, dihydroxymethylpropionic acid, tris(2-hydroxyethyl)methyl sulfate, zinc citrate, monosodium citrate or disodium citrate, or a combination of at least two thereof.

4. The ionic polyurethane composition according to claim 1, characterized in that The polyether polyol A and the polyether polyol B independently include any one of polymer polyol, polypropylene glycol or polytetramethylene glycol or a combination of at least two thereof.

5. The ionic polyurethane composition according to claim 1, characterized in that The number average molecular weights of the polyether polyol A and the polyether polyol B are independently 1000 to 6000.

6. The ionic polyurethane composition according to claim 1, characterized in that The functionality of the polyether polyol A and the polyether polyol B are independently 2 to 3.

7. The ionic polyurethane composition according to claim 4, characterized in that The number average molecular weight of the polytetrahydrofuran diol is 1000-3000.

8. The ionic polyurethane composition according to claim 1, characterized in that The mass ratio of solute to water in the aqueous solution containing ionic groups is 1:(2-4).

9. The ionic polyurethane composition according to claim 1, characterized in that The catalyst includes an organotin catalyst.

10. The ionic polyurethane composition according to claim 1, characterized in that: The ionic composition further comprises silicone oil and / or color paste.

11. The ionic polyurethane composition according to claim 10, characterized in that: The content of silicone oil in the ionic composition is 1 to 2 parts by weight.

12. The ionic polyurethane composition according to claim 10, characterized in that: The content of the color paste in the ionic composition is 2 to 4 parts by weight.

13. A method for preparing the ionic polyurethane composition according to any one of claims 1 to 12, characterized in that: The preparation method comprises preparing an ionic prepolymer and preparing an ionic composition respectively; The preparation method of the ionic prepolymer comprises: reacting polyether polyol A and part of polyisocyanate, adding a compound containing an ionic group capped with an active group to react, and then adding the remaining part of polyisocyanate to mix, thereby obtaining the ionic prepolymer; The preparation method of the ionic composition comprises: mixing polyether polyol B, an aqueous solution containing ionic groups, a chain extender, a catalyst, optionally silicone oil and optionally color paste to obtain the ionic composition.

14. The preparation method according to claim 13, characterized in that: The reaction time of the polyether polyol A and part of the polyisocyanate is 3 to 6 hours.

15. The preparation method according to claim 13, characterized in that: The reaction temperature of the polyether polyol A and part of the polyisocyanate is 60-100°C.

16. The preparation method according to claim 13, characterized in that: The reaction time of adding active groups to cap the compounds containing ionic groups is 2 to 4 hours.

17. The preparation method according to claim 13, characterized in that: The reaction temperature for the reaction of adding active groups to cap the ionic group-containing compound is 60-100°C.

18. The preparation method according to claim 13, characterized in that: The adding of the remaining part of the polyisocyanate for mixing is carried out at a temperature below 60°C.

19. The preparation method according to claim 13, characterized in that: The mixing time for adding the remaining part of the polyisocyanate is 5 to 20 minutes.

20. The preparation method according to claim 13, characterized in that: The mixing time of the polyether polyol B, the aqueous solution containing ionic groups, the chain extender, the catalyst, the optional silicone oil and the optional color paste is 0.5 to 1 hour.

21. An ionic polyurethane elastomer, characterized in that: The raw materials for preparing the ionic polyurethane elastomer include the ionic polyurethane composition according to any one of claims 1 to 12.

22. A method for preparing the ionic polyurethane elastomer according to claim 21, characterized in that: The preparation method comprises: mixing the ionic prepolymer in the ionic polyurethane composition according to any one of claims 1 to 12 with the ionic composition, and curing and foaming the mixture to obtain the ionic polyurethane elastomer.

23. An ionic polyurethane tire, characterized in that: The raw materials for preparing the ionic polyurethane tire include the ionic polyurethane composition according to any one of claims 1 to 12.

24. The ionic polyurethane tire according to claim 23, characterized in that: The ionic polyurethane tire is an ionic polyurethane bicycle tire.

25. The ionic polyurethane tire according to claim 23, characterized in that: The density of the ionic polyurethane tire is 500-600 kg / m 3 .

26. A method for preparing an ionic polyurethane tire as claimed in any one of claims 23 to 25, characterized in that: The preparation method comprises: mixing the ionic prepolymer and the ionic composition in the ionic polyurethane composition according to any one of claims 1 to 12, pouring them into a mold, and curing and foaming them to obtain the ionic polyurethane tire.

27. The preparation method according to claim 26, characterized in that: The mass ratio of the ionic prepolymer to the ionic composition is (0.7-1.3):

1.

28. The preparation method according to claim 26, characterized in that: The temperature of the mold is 45-65°C.

29. The preparation method according to claim 26, characterized in that: The rotation speed of the mold is 500-800 m / min.

30. The preparation method according to claim 26, characterized in that: The method further comprises the step of opening the mold after the curing and foaming.

31. The preparation method according to claim 30, characterized in that: The mold opening time is 3 to 10 minutes.

Citation Information

Patent Citations

  • Thermoplastic polyurethane elastomer with ultralow temperature resistance and high mechanical property and preparation method of thermoplastic polyurethane elastomer

    CN113980232A

  • Method for manufacturing polyurethane microporous automotive buffer block

    CN101838458A

  • Transparent polyurethane elastomer and preparation method as well as application

    CN102604038A

  • B component isocyanate prepolymer and polyurethane double components for preparing microcellular polyurethane elastomer and application

    CN105949434A

  • Polyurethane elastomer composite material used for tyre filling, and preparation method and applications thereof

    CN108164991A