A lithium removal method without hydrogen generation

By using an anhydrous reagent to react with lithium battery waste, the generation of hydrogen is avoided, the problem of safety risks in the treatment of lithium battery waste is solved, and the effective recovery of resources is achieved.

CN115725841BActive Publication Date: 2024-10-18CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202110985123.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-25
Publication Date
2024-10-18
Estimated Expiration
2041-08-25

AI Technical Summary

Technical Problem

In the existing lithium battery waste treatment methods, metallic lithium reacts with water to produce hydrogen, which has flammable and explosive safety issues, and it is difficult to effectively solve the risk of hydrogen accumulation and explosion.

Method used

An anhydrous reagent, such as polysulfide Li2Sx, nitrogen, sulfur dioxide or chlorine, is used to react the metallic lithium waste with the anhydrous reagent through a heated reactor to avoid the generation of hydrogen and recover metallic lithium through electrolysis.

Benefits of technology

It achieves the production of no hydrogen when processing metallic lithium waste, reduces safety risks, allows metallic lithium and other by-products to be effectively recycled, and reduces harm to the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115725841B_ABST
    Figure CN115725841B_ABST
Patent Text Reader

Abstract

The present invention discloses a lithium removal method without hydrogen generation, comprising: placing metal lithium waste in a reactor; adding an anhydrous reactant selected from a compound solid phase reactant, a gas phase reactant and a metal phase reactant into the reactor; heating the reactor to react the metal lithium waste with the anhydrous reactant. The lithium removal method of the present invention is safe, non-combustion and non-explosion, and the metal lithium and other byproducts after treatment can be further recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery waste treatment and resource recovery, and in particular to a lithium removal method without generating hydrogen. Background Art

[0002] Lithium-ion batteries have been widely used as energy storage devices in information technology, electric vehicles, aerospace and other fields due to their high energy density, high voltage, good cycle performance and low self-discharge. With the popularization of lithium-ion batteries, the treatment of lithium battery waste has also received increasing attention.

[0003] But overall, current methods of treating lithium metal waste generally present significant safety risks. Summary of the invention

[0004] In order to solve all or part of the above problems, the present invention provides a lithium removal method without hydrogen generation, which can effectively solve the safety problems existing in the treatment process of waste containing metallic lithium.

[0005] Specifically, the present invention is achieved through the following technical solutions:

[0006] A lithium removal method without hydrogen generation, comprising:

[0007] Placing waste containing metallic lithium in a reactor;

[0008] Adding an anhydrous reactant selected from a compound solid phase reactant, a gas phase reactant and a metal phase reactant into the reaction furnace;

[0009] The reaction furnace is heated to cause the waste containing metallic lithium and the anhydrous reactant to react.

[0010] Optionally, in the process of heating the reaction furnace, the heating temperature is 80° C. to 1000° C., and the heating time is 1 minute to 3 hours.

[0011] Optionally, the anhydrous reactant is a compound solid phase reactant; preferably, the compound solid phase reactant is a polysulfide Li2S x ; More preferably, x is 2, 4 or 6.

[0012] Optionally, the compound solid phase reactant is added to the reaction furnace according to a molar ratio of the compound solid phase reactant to lithium in the waste containing metallic lithium of 1:(2-10).

[0013] Optionally, in the process of heating the reaction furnace, the heating temperature is 80° C. to 100° C., the heating time is 30 minutes to 3 hours and preferably 2 to 3 hours.

[0014] Optionally, the anhydrous reactant is a gas phase reactant; preferably, the gas phase reactant is any one of nitrogen, sulfur dioxide and chlorine.

[0015] Optionally, gas-phase reactants are introduced into the reactor at a rate of 2L / min to 10L / min and preferably 5L / min to 10L / min; during the heating of the reactor, the heating temperature is 80°C to 100°C, the heating time is 1 minute to 1 hour and preferably 0.5 to 1 hour.

[0016] Optionally, the safe lithium removal method without hydrogen generation also includes: electrolyzing the reactants obtained by reacting the metallic lithium-containing waste with the anhydrous reactant; returning the gas obtained by electrolysis to the reactor, and / or recovering the metallic lithium obtained by electrolysis.

[0017] Optionally, the anhydrous reactant is a metal phase reactant; preferably, the metal phase reactant is any metal except iron.

[0018] Optionally, in the process of heating the reaction furnace, the heating temperature is 100° C. to 1000° C. and preferably 600° C. to 1000° C., and the heating time is 2 to 3 hours.

[0019] Compared with the prior art, the lithium removal method without hydrogen generation of the present invention has at least the following beneficial effects:

[0020] The lithium removal method without hydrogen generation of the present invention adopts an anhydrous reactant as the reactant, thereby avoiding the safety problems such as flammability and explosion caused by the violent reaction between metallic lithium and water and the generation of hydrogen.

[0021] By adopting the lithium removal method without hydrogen generation of the present invention, the treated metallic lithium and other by-products can be recycled, which not only reduces the harm to the environment but also effectively recycles resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:

[0023] Figure 1 A flow chart of the lithium removal method without hydrogen generation of the present invention is shown.

[0024] Figure 2 A flow chart showing a lithium removal method using lithium polysulfide in a preferred embodiment of the present invention.

[0025] Figure 3 A flow chart showing a lithium removal method using a gas phase reactant in another preferred embodiment of the present invention.

[0026] Figure 4 A flow chart showing a lithium removal method using a metal other than iron in another preferred embodiment of the present invention. DETAILED DESCRIPTION

[0027] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific implementation methods, but the present invention is not limited thereto.

[0028] The inventors found that among the existing metal lithium recovery technologies for lithium batteries, common technologies include, for example, the Chinese invention patent application with application number 201711130452.1, which discloses a lithium recovery and reuse process. This method uses chemical precipitation to remove lithium, cools down with liquid nitrogen, reduces the reactivity of lithium, and pulverizes the cooled components and reacts with water to precipitate lithium compounds; the lithium salt is dissolved in low-concentration sulfuric acid, so that it can be further purified, and the LiOH produced in the reaction can finally be converted into LiCO3 and precipitated. However, during the synthesis of lithium compounds, lithium and water will react violently and produce hydrogen, which poses a safety problem of being flammable and explosive.

[0029] Another example is the Chinese invention patent application with application number 201510144800.5, which discloses a sodium-potassium-lithium and lithium slag waste treatment device. The treatment device slowly presses the lithium slag into the hydrolysis pump through the lithium slag metering pump, and undergoes a hydrolysis reaction with a large amount of water in the hydrolysis pump; the reaction heat generated in the reaction is taken away by the cooling water of the kettle jacket, which can prevent overheating and overpressure, and the hydrolysis temperature will not fluctuate greatly. However, metallic lithium is very active, and in the presence of a large amount of water, it will quickly undergo a hydrolysis reaction to produce a large amount of hydrogen; even if the reaction temperature is controlled by controlling the reaction amount and reaction speed of the lithium slag, the explosion risk caused by hydrogen accumulation cannot be solved.

[0030] In view of the safety issues existing in the current treatment process of lithium-containing waste, the present invention provides a lithium removal method without hydrogen generation, such as Figure 1 As shown, the method comprises the following steps:

[0031] Step S1: placing metallic lithium waste in a reactor.

[0032] The lithium removal method of the present invention has universal applicability and can be applied to any type of metal lithium waste. Specifically, the lithium removal method of the present invention is applicable to pure metal lithium waste, such as lithium scraps, lithium belt scraps, etc.; in addition, the lithium removal method of the present invention is also applicable to lithium-containing pole piece waste, such as carbon system lithium-containing anode piece waste, silicon system lithium-containing anode piece waste, etc.

[0033] The lithium removal method of the present invention has no special requirements on the reaction furnace, and those skilled in the art can select any conventional reaction furnace to implement the lithium removal method of the present invention according to actual needs.

[0034] Step S2: adding an anhydrous reactant selected from a compound solid phase reactant, a gas phase reactant and a metal phase reactant into the reaction furnace.

[0035] Preferably, the compound solid phase reactant is polysulfide Li2S x More preferably, x is 2, 4 or 6. The inventors have found through research that the use of polysulfide to remove lithium from metal lithium waste is mild in the whole process, does not produce flammable gases such as hydrogen, and eventually forms lithium sulfate, which can be recycled.

[0036] Preferably, the gas phase reactant is any one of nitrogen, sulfur dioxide and chlorine. The inventors have found through research that the use of nitrogen, sulfur dioxide or chlorine to remove lithium from metal lithium waste has a fast reaction speed and does not produce flammable gases such as hydrogen. The corresponding lithium compounds produced can be converted into metal lithium and corresponding gases through electrolysis, thereby achieving recovery.

[0037] Preferably, the metal phase reactant is any metal except iron. The inventors have found through research that the lithium removal treatment of metal lithium waste by fusing metals other than iron with metal lithium waste is an in-situ reaction and does not produce flammable gases such as hydrogen. In addition, the treatment method is simple to operate, has a large production capacity, can directly form an alloy, and has a high economic benefit.

[0038] Step S3: heating the reaction furnace to react the waste containing metallic lithium with the anhydrous reactant. The heating temperature is selected to be any temperature within the range of 80° C. to 1000° C. or any temperature within a range of temperatures, and the heating time is 1 minute to 3 hours.

[0039] The present invention will be further described in detail below with reference to the accompanying drawings for three situations: compound solid phase reactant, gas phase reactant and metal phase reactant.

[0040] Figure 2 The flowchart of a lithium removal method using lithium polysulfide provided by a preferred embodiment of the present invention is shown. In this embodiment, graphite system pole piece waste (i.e., graphite system waste pole piece) is used as an example for explanation. It can be understood by those skilled in the art that this is only exemplary, and the lithium removal method in this embodiment is also applicable to pure metal lithium waste such as lithium chips, lithium belt scraps, or other pole piece waste such as silicon system lithium-containing anode piece waste. Figure 2 As shown, the lithium removal method comprises the following steps:

[0041] Step S101: Place the waste graphite system electrode sheets in a reaction furnace.

[0042] In order to ensure the full reaction of metallic lithium, the waste graphite system electrode sheets are cut in advance. The specific cutting size can be reasonably selected by those skilled in the art according to actual needs. After cutting, it can ensure that all positions of the waste electrode sheets are in contact with the reactant, thus ensuring the full reaction of metallic lithium.

[0043] Step S102: Add lithium polysulfide to the reaction furnace.

[0044] The lithium polysulfide used in the present invention can be Li2S2, Li2S4 or Li2S6. The molar ratio of the added lithium polysulfide to the metallic lithium in the waste graphite system electrode sheets is 1:(2 - 10). For example, when the lithium polysulfide is Li2S2, the molar ratio of Li2S2 to the metallic lithium in the waste graphite system electrode sheets can be 1:2; when the lithium polysulfide is Li2S4, the molar ratio of Li2S2 to the metallic lithium in the waste graphite system electrode sheets can be 1:(2 - 4); when the lithium polysulfide is Li2S6, the molar ratio of Li2S2 to the metallic lithium in the waste graphite system electrode sheets can be 1:(2 - 10).

[0045] Step S103: Heat the reaction furnace to cause the waste graphite system electrode sheets to react with lithium polysulfide.

[0046] The temperature used for heating the reaction furnace is 80°C - 100°C, and the heating time of the reaction furnace is 30 minutes to 3 hours, and preferably 2 - 3 hours.

[0047] The chemical properties of lithium polysulfide are relatively active. Under heating conditions, lithium polysulfide will react with the metallic lithium in the waste graphite system electrode sheets to form lithium sulfide. Because the chemical properties of lithium polysulfide are relatively active, the reaction can occur only by heating to 80°C - 100°C, and the reaction conditions are mild. Further, lithium sulfide will form lithium sulfate when continuously heated in oxygen. The reaction in the whole process is mild and no flammable gas such as hydrogen will be generated.

[0048] This step mainly involves the following chemical reactions:

[0049] Li2S x +(2x - 2)Li → x Li2S (x = 2, 4 or 6)

[0050] Li2S + 2O2 → Li2SO4

[0051] Step S104: Recover lithium sulfate.

[0052] The specific recovery method can be any conventional method, and those skilled in the art can make a reasonable choice according to needs, which will not be described in detail here.

[0053] Figure 3 The flowchart of a lithium removal method using a gas phase reactant provided by a preferred embodiment of the present invention is shown. In this embodiment, graphite system pole piece waste is used as an example for explanation. Those skilled in the art will understand that this is only exemplary, and the lithium removal method in this embodiment is also applicable to pure metal lithium waste such as lithium chips, lithium ribbon scraps, or other pole piece waste such as silicon system lithium-containing anode sheet waste. Figure 3 As shown, the lithium removal method comprises the following steps:

[0054] Step S201: placing the graphite system waste electrode sheets in a reaction furnace.

[0055] In order to ensure that the metal lithium fully reacts, the graphite system waste electrode pieces are cut in advance, and the specific cutting size can be reasonably selected by those skilled in the art according to actual needs. After the cutting process, it can be ensured that each position of the waste electrode piece is in contact with the reactant, thereby ensuring that the metal lithium fully reacts.

[0056] Step S202: introducing gas-phase reactants into the reaction furnace.

[0057] The gas phase reactant used in the present invention is any one of nitrogen, sulfur dioxide and chlorine. The speed of introducing the gas phase reactant into the reaction furnace is 2L / min to 10L / min, and preferably 5L / min to 10L / min.

[0058] Step S203: heating the reaction furnace to allow the graphite system electrode waste to react with the gas phase reactant.

[0059] The temperature used for heating the reaction furnace is 80° C. to 100° C., and the heating time for the reaction furnace is 1 minute to 1 hour, and preferably 0.5 to 1 hour.

[0060] When using nitrogen, sulfur dioxide or chlorine to remove lithium from graphite electrode waste, the reaction speed is fast. It only needs to be heated to 80℃~100℃ to make nitrogen, sulfur dioxide or chlorine react quickly with metallic lithium to produce corresponding lithium compounds. The whole process is mild and does not produce flammable gases such as hydrogen.

[0061] This step mainly involves the following chemical reactions:

[0062] N2+2Li→2LiN

[0063] SO2+2Li→Li2S+O2

[0064] Cl2+2Li→2LiCl

[0065] Step S204: electrolyze the reaction product and transport the obtained gas back to the reaction furnace.

[0066] During the electrolysis of the reaction product, the electrolysis temperature is 30°C to 70°C, preferably 60°C to 70°C, and the current density is 1 to 3 KA / m 3 , preferably 2~3KA / m 3 .

[0067] The electrolytic treatment in this step mainly involves the following chemical reactions:

[0068] 2LiN→N2+2Li

[0069] Li2S+O2→SO2+2Li

[0070] 2LiCl→Cl2+2Li

[0071] The gas obtained by electrolysis is transported back to the reactor and reused to react with the graphite system electrode waste.

[0072] Step S205: recovering the metallic lithium obtained by electrolysis.

[0073] The specific recycling method can be carried out by conventional methods, which will not be described in detail here.

[0074] The above-mentioned step S204 and step S205 are optional steps of the embodiment of the present invention, and there is no strict order between the two. After the electrolysis treatment, the gas and the metallic lithium can be recovered simultaneously or sequentially.

[0075] Figure 4 The flowchart of a lithium removal method using metals other than iron provided by a preferred embodiment of the present invention is shown. In this embodiment, graphite system pole piece waste is used as an example for explanation. Those skilled in the art will understand that this is only exemplary, and the lithium removal method in this embodiment is also applicable to pure metal lithium waste such as lithium scraps, lithium ribbon scraps, or other pole piece waste such as silicon system lithium-containing anode sheet waste. Figure 4 As shown, the lithium removal method comprises the following steps:

[0076] Step S301: placing the graphite system waste electrode sheets in a reaction furnace.

[0077] In order to ensure that the metal lithium fully reacts, the graphite system waste electrode pieces are cut in advance, and the specific cutting size can be reasonably selected by those skilled in the art according to actual needs. After the cutting process, it can be ensured that each position of the waste electrode piece is in contact with the reactant, thereby ensuring that the metal lithium fully reacts.

[0078] Step S302: adding metals other than iron into the reaction furnace.

[0079] The inventors have found through research that metallic iron is difficult to fuse with metallic lithium, so the present invention does not use iron. Other metals can be used in the present invention, for example, aluminum, magnesium, zinc, copper, etc.

[0080] The present invention has no special requirements for the amount of metal, as long as it can be fused with the waste electrode sheet. Those skilled in the art can make a reasonable choice according to actual conditions.

[0081] Step S303: heating the reaction furnace to allow the graphite system waste electrode to react with the metal.

[0082] The temperature used for heating the reaction furnace is 100°C to 1000°C, preferably 600°C to 1000°C, and the heating time of the reaction furnace is 2 to 3 hours.

[0083] The reaction between metal and graphite waste electrode sheets under high temperature conditions is an in-situ reaction, and no flammable gas such as hydrogen is produced during the reaction. In addition, this treatment method is simple to operate, has a large production capacity, can directly form an alloy, and has high economic benefits.

[0084] Step S304: purifying metallic lithium.

[0085] The material obtained by the heating reaction is an alloy of carbon, electrode (copper foil), metal, and lithium. For example, when aluminum and graphite waste electrode are heated for reaction, a carbon-copper-aluminum-lithium alloy is obtained.

[0086] The alloy can be further used to purify lithium. The specific purification method can be carried out by conventional methods, which will not be described in detail here.

[0087] Example

[0088] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are selected according to conventional methods and conditions.

[0089] Examples 1 to 5 and Comparative Examples 1 to 5

[0090] 100 g of graphite waste electrode with lithium film was processed. Specific parameters are shown in Table 1.

[0091] Effect detection:

[0092] (1) Amount of hydrogen produced during the reaction: A hydrogen concentration detector was used to detect the real-time hydrogen concentration produced during the reaction.

[0093] (2) Recovery rate of lithium sulfate: 1-2 g of the final product sample is digested in a mixed acid (hydrochloric acid + nitric acid) solution and diluted 50-150 times. Its absorbance is measured at 670.78 nm in the atomic spectrum and compared with the standard absorbance curve of lithium ions to find out the lithium ion concentration and calculate the recovery rate of lithium sulfate salt.

[0094] (3) Copper electrode recovery rate: The copper foil recovery rate is calculated by using the theoretical copper foil weight of the electrode to be processed ÷ the actual copper foil weight recovered × 100%.

[0095] Table 1

[0096]

[0097] It can be seen from the data in Table 1 that according to the method of the present invention, when polysulfide is used to remove lithium from waste electrode sheets with lithium film, no hydrogen is generated during the whole process, and the recovery rate of lithium sulfate produced as a byproduct during the reaction process can reach more than 83%, and the recovery rate of copper electrode sheets can reach more than 80%. However, if the material ratio of the present invention is not adopted (Comparative Example 1), the reaction time of the present invention is not adopted (Comparative Example 2), the heating temperature conditions of the present invention are not adopted (Comparative Examples 3 and 4), or the polysulfide of the present invention is not used for lithium removal (Comparative Example 5), the byproduct recovery rate of the present invention cannot be achieved or no hydrogen is generated during the whole process cannot be achieved.

[0098] Examples 6 to 10 and Comparative Examples 6 to 10

[0099] 100 g of graphite waste electrode with lithium film was processed. See Table 2 for specific parameters.

[0100] Effect detection:

[0101] (1) Amount of hydrogen produced during the reaction: A hydrogen concentration detector was used to detect the real-time hydrogen concentration produced during the reaction.

[0102] (2) Lithium metal treatment rate: The treated electrode samples are placed in water, and the gas generated by the residual lithium in the electrode and the water is collected using the drainage method. The amount of residual lithium metal can be calculated from the gas volume, thereby calculating the lithium metal treatment rate.

[0103] (3) Copper electrode recovery rate: The copper foil recovery rate is calculated by using the theoretical copper foil weight of the electrode to be processed ÷ the actual copper foil weight recovered × 100%.

[0104] Table 2

[0105]

[0106] It can be seen from the data in Table 2 that according to the method of the present invention, when nitrogen, sulfur dioxide or chlorine is used to remove lithium from waste pole pieces with lithium film, the treatment rate of metallic lithium can reach more than 90%, no hydrogen is generated during the whole process, and the recovery rate of copper pole pieces can reach more than 80%. However, although the gas (nitrogen) used in the present invention is used, but the gas flow rate of the present invention (Comparative Example 6), the treatment time of the present invention (Comparative Example 7), and the heating temperature of the present invention (Comparative Examples 8 and 9) are not used, the lithium removal rate or copper pole piece recovery rate of the present invention cannot be achieved, or, although the process conditions and parameters of the present invention are used, but the gas of the present invention is not used (Comparative Example 10), the effect of no hydrogen generation during the whole process cannot be achieved.

[0107] Examples 11 to 13 and Comparative Example 11

[0108] 100 g of graphite waste electrode with lithium film was processed. See Table 3 for specific parameters.

[0109] Effect detection:

[0110] (1) Amount of hydrogen produced during the reaction: A hydrogen concentration detector was used to detect the real-time hydrogen concentration produced during the reaction.

[0111] (2) Alloy yield: The lithium content in the product alloy tested by atomic absorption spectroscopy is ÷ the metal lithium content of the actual processed electrode × 100%.

[0112] Table 3

[0113]

[0114] It can be seen from the data in Table 3 that when metals other than iron are used to remove lithium from waste electrodes with lithium film, a 100% lithium alloy yield can be achieved while ensuring that no hydrogen is generated during the entire process.

[0115] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other substitutions, modifications, combinations, changes, simplifications, etc. made without departing from the spirit and principles of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A lithium removal method without hydrogen generation, characterized in that: include: Placing waste containing metallic lithium in a reactor; Adding an anhydrous reactant selected from a compound solid phase reactant, a gas phase reactant and a metal phase reactant into the reaction furnace; The reaction furnace is heated to allow the waste containing metallic lithium to react with the anhydrous reactant. The anhydrous reactant is a compound solid phase reactant, a gas phase reactant or a metal phase reactant, The compound solid phase reactant is polysulfide Li2S x ; The gas phase reactant is any one of nitrogen, sulfur dioxide and chlorine; The metal phase reactant is any metal except iron.

2. The lithium removal method without hydrogen generation according to claim 1, characterized in that: In the process of heating the reaction furnace, the heating temperature is 80° C. to 1000° C., and the heating time is 1 minute to 3 hours.

3. The lithium removal method without hydrogen generation according to claim 1 or 2, characterized in that: x is 2, 4, or 6.

4. The lithium removal method without hydrogen generation according to claim 3, characterized in that: The compound solid phase reactant is added into the reaction furnace according to the molar ratio of the compound solid phase reactant to the lithium in the waste containing metallic lithium being 1:(2-10).

5. The lithium removal method without hydrogen generation according to claim 1, characterized in that: In the process of heating the reaction furnace, the heating temperature is 80° C. to 100° C., and the heating time is 30 minutes to 3 hours.

6. The lithium removal method without hydrogen generation according to claim 5, characterized in that: The heating time is 2 to 3 hours.

7. The lithium removal method without hydrogen generation according to claim 1, characterized in that: The gas phase reactant is introduced into the reaction furnace at a rate of 2L / min to 10L / min; in the process of heating the reaction furnace, the heating temperature is 80°C to 100°C, and the heating time is 1 minute to 1 hour.

8. The lithium removal method without hydrogen generation according to claim 7, characterized in that: The gas phase reactant is introduced into the reaction furnace at a rate of 5 L / min to 10 L / min.

9. The lithium removal method without hydrogen generation according to claim 7, characterized in that: The heating time is 0.5 to 1 hour.

10. The lithium removal method without hydrogen generation according to claim 1, characterized in that: The lithium removal method without hydrogen generation also includes: electrolyzing a reactant obtained by reacting the waste containing metallic lithium with the anhydrous reactant; The gas obtained by electrolysis is returned to the reactor, and / or the metallic lithium obtained by electrolysis is recovered.

11. The lithium removal method without hydrogen generation according to claim 1, characterized in that: In the process of heating the reaction furnace, the heating temperature is 100° C. to 1000° C., and the heating time is 2 to 3 hours.

12. The lithium removal method without hydrogen generation according to claim 11, characterized in that: The heating temperature is 600°C to 1000°C.

Citation Information

Patent Citations

  • A device for treating sodium, potassium, lithium and lithium slag waste

    CN104764024B

  • Lithium recycling process

    CN108011145A

  • Method of making high purity lithium hydroxide and hydrochloric acid

    CA2725443A1

  • Process for the recovery of lithium from waste lithium ion batteries

    CA3144711A1