Treatment liquid composition for dye printing, composition set, printing and dyeing method, and inkjet printing and dyeing method
By using a treatment liquid composition of polyester resin with a high glass transition temperature and a crosslinker on the natural fiber fabric, and combining inkjet printing and dyeing technology, the problem of insufficient color development and firmness of the natural fiber fabric is solved, and the problem of insufficient color development and firmness of the natural fiber fabric is achieved. High color rendering and durability printing effect.
Patent Information
- Application Number
- CN202211034546.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-08-26
AI Technical Summary
The prior art is difficult to achieve sufficient color development and firmness on natural fiber fabrics, especially when using a pretreatment liquid, it is difficult to obtain excellent color discoloration and fading properties and friction resistance.
Using a treatment liquid composition containing a polyester resin with a glass transition temperature of 40°C or above and a crosslinking agent, the ink composition is imparted to disperse dye and water to achieve polymerization by adhering it to the cloth and combining inkjet printing and dyeing method. The crystallization and bonding of the ester resin enhances the adhesion and durability of the dye.
The color rendering, color discoloration and friction resistance of natural fiber fabrics are achieved, and the firmness and texture of the printing dyes are ensured, and the color rendering and durability of the printing materials are improved.
Smart Images

Figure BDA0003818626220000231 
Figure BDA0003818626220000241 
Figure BDA0003818626220000261
Abstract
Description
Technical Field
[0001] The present invention relates to a treatment liquid composition for dye printing and dyeing, a composition group, a printing and dyeing method and an inkjet printing and dyeing method. Background Art
[0002] Conventionally, when dyeing a cloth with a color material to produce a printed article, a technique of pre-treating the cloth with a treatment liquid is known in order to improve the color development and fastness of the color material. As such a technique, for example, Patent Document 1 discloses a technique of attaching a pre-treatment liquid composed of an aqueous composition to a polyester cloth.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-249773
[0006] However, Patent Document 1 is a technology for polyester fabrics, and does not describe printing and dyeing for natural fiber fabrics. Polyester fabrics are different from natural fiber fabrics in that they can be printed and dyed using dyes even without using a pretreatment liquid, and the resulting printed and dyed products generally have color development and fastness. However, even if the pretreatment liquid of Patent Document 1 is used for natural fiber fabrics, the pretreatment liquid has a technical problem that it is difficult to obtain printed and dyed products with sufficient color development, fastness, and color change and fading resistance. Summary of the invention
[0007] The present invention provides a dye printing treatment liquid composition which is used by attaching it to a fabric, and contains a polyester resin having a glass transition temperature of 40° C. or higher, a crosslinking agent, and water. The fabric contains fibers having a hydroxyl group. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 This is a flowchart showing an example of the indirect dye printing recording method according to the present embodiment. DETAILED DESCRIPTION
[0009] Hereinafter, an embodiment of the present invention (hereinafter referred to as “the present embodiment”) will be described in detail, but the present invention is not limited thereto and various modifications can be made without departing from the gist of the invention.
[0010] 1. Treatment liquid composition for dye printing
[0011] The dye printing treatment liquid composition of this embodiment (hereinafter also referred to as "treatment liquid composition") is attached to a fiber fabric having a hydroxyl group before dye printing. The treatment liquid composition contains a polyester resin having a glass transition temperature of 40°C or higher, a crosslinking agent, and water.
[0012] According to this embodiment, by pre-attaching the treatment liquid composition to a cloth containing fibers having hydroxyl groups, and then dyeing the cloth to which the treatment liquid composition is attached, it is possible to simply obtain a printed material having sufficient color development, color change and fading resistance over time, and resistance to friction.
[0013] The reason why such excellent effects are obtained by this embodiment is not certain, but the present inventors speculate as follows.
[0014] That is, the ink containing disperse dyes and the like, which are usually used for printing and dyeing, has low affinity for fabrics such as cotton containing fibers having hydroxyl groups, and is not easy to perform dye printing and dyeing. On the other hand, the ink containing disperse dyes and the like easily dyes polyester resins through hydrogen bonds with carboxyl groups, π-π interactions with hydrophobic parts such as phenyl groups, and non-covalent bonds such as van der Waals forces in the structure of polyester resins. Moreover, polyester resins have high affinity for fabrics containing fibers, so they can exist on fabrics. Therefore, by using a treatment agent composition to attach polyester resins to fabrics, it is possible to impart dyeability of ink containing disperse dyes and the like even to fibers having hydroxyl groups such as cotton.
[0015] However, in the structure of polyester resin, when there are few hydrophobic parts or crystallization with fabrics has not been carried out, disperse dyes are not easy to dye non-crystalline parts, so it is not easy to dye polyester resins, and printed fabrics are easy to fade over time. On the other hand, the treatment liquid composition of this embodiment contains a polyester resin with a glass transition temperature of 40°C or more. Therefore, the polyester resin can be crystallized on the fabric, and the disperse dye can impart ink to the crystalline part of the polyester resin. Therefore, according to this embodiment, sufficient color development can be imparted, and excellent color change and fading properties of printed fabrics can be imparted over time.
[0016] On the other hand, polyester resin only adheres to the fabric but does not adhere to the fabric. Therefore, by using a polyester resin with a glass transition temperature of 40°C or more, even if sufficient color development and excellent color change and fading properties can be obtained, the fastness such as friction resistance will be insufficient. In this regard, in the treatment liquid composition of this embodiment, since a cross-linking agent is contained, the polyester resin can be bonded to the fabric. Therefore, according to this embodiment, it is presumed that a printed and dyed product having both sufficient color development and excellent color change and fading properties and excellent fastness can be obtained. However, the reason is not limited to this.
[0017] Next, each component contained in the treatment liquid composition will be described, and the fabric will be described later.
[0018] 1.1. Polyester resin with a glass transition temperature of 40°C or above
[0019] The treatment liquid composition contains a polyester resin having a glass transition temperature of 40° C. or higher.
[0020] By including the polyester resin in the treatment liquid composition, a printed textile having sufficient color development and excellent color change and fading properties can be obtained.
[0021] The polyester resin is not particularly limited as long as it has a glass transition temperature of 40° C. or higher. In the present embodiment, the glass transition temperature of the polyester resin can be measured, for example, by a differential scanning calorimeter (hereinafter also referred to as “DSC”).
[0022] When printing and dyeing the fabric to which the treatment liquid composition is attached, a printed product having more sufficient color development, color change and fading resistance, and fastness can be obtained, so the glass transition temperature is preferably 50°C or higher. The lower limit is, for example, 180°C or lower, and may be 150°C or lower.
[0023] The polyester resin has, for example, a structural unit derived from a polyvalent carboxylic acid and a structural unit derived from a polyol.
[0024] Examples of the polycarboxylic acid include terephthalic acid, isophthalic acid, phthalic acid, phthalic acid, 4,4′-diphenyldicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 2-potassium sulfoterephthalate, 5-sodium sulfoisophthalate, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, succinic anhydride, and p-hydroxybenzoic acid, and salts thereof. Examples of the salt include potassium salts, sodium salts, calcium salts, and magnesium salts.
[0025] Examples of the polyol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, terephthalic acid, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyoxytetramethylene glycol, dimethylolpropionic acid, glycerol, trimethylolpropane, sodium dimethylolethylsulfonate, potassium dimethylolethylsulfonate, and potassium dimethylolpropionate.
[0026] The polyester resin preferably contains a hydroxyl group, a carboxyl group, a sulfonic acid group, and sodium salts thereof. These groups may be contained alone or in combination of two or more.
[0027] The sulfonic acid group-containing polyester resin has, for example, a structural unit derived from a polycarboxylic acid, a structural unit derived from a polyol, and a structural unit derived from a sulfonic acid-containing aromatic monomer.
[0028] Examples of the sulfonic acid-containing aromatic monomer include 5-sulfoisophthalic acid, sulfoterephthalic acid, 4-sulfophthalic acid, 4-sulfonaphthalene-2,7-dicarboxylic acid, 4-sulfo-1,8-naphthalene dicarboxylic anhydride, and salts thereof. The salts mentioned above may be used as the salts, and sodium salts are preferred.
[0029] By containing these groups, the polyester resin can react well with the crosslinking agent and have good adhesion with the fabric containing the fiber having the hydroxyl group. Therefore, a printed product having further sufficient color development, color change and fading resistance, and fastness can be obtained.
[0030] From the viewpoint of more sufficient color development and more excellent color change and fading resistance, the polyester resin preferably contains a hydrophobic portion such as an aromatic portion in its structure.
[0031] The polyester resin can be obtained by, for example, appropriately selecting one or more from each of the above-mentioned polycarboxylic acids, polyols, and, if necessary, sulfonic acid-containing aromatic monomers, and synthesizing them by a conventional polycondensation reaction.
[0032] As such polyester resin, commercially available products may also be used. Commercially available products include, for example, Plascoat (registered trademark) Z-221, Z-446, Z-561, Z-565, RZ-570, Z-592, Z-687, Z-690, Z-730, Z-760, RZ-105, RZ-570 and RZ-760 (the above are trade names, manufactured by Huying Chemical Industry Co., Ltd.); Vylonal (registered trademark) MD-1200, MD-1500 and MD-2000 (the above are trade names, manufactured by Toyobo Co., Ltd.).
[0033] The polyester resins may be used alone or in combination of two or more.
[0034] From the perspective of obtaining a printed product with more sufficient color development, color change and fading properties, and fastness, the content of the polyester resin is preferably 0.5 to 12.5% by mass relative to the total amount of the treatment liquid composition in terms of solid content conversion. From the perspective of obtaining a printed product with more sufficient color development and color change and fading properties, and having better fastness, the content of the polyester resin is more preferably 1.5 to 8.0% by mass relative to the total amount of the treatment liquid composition in terms of solid content conversion. From the perspective of obtaining a printed product with more sufficient color development, color change and fading properties, and fastness, and having good texture, the content of the polyester resin is more preferably 1.0 to 6.0% by mass relative to the total amount of the treatment liquid composition in terms of solid content conversion. From the perspective of obtaining a printed product with more sufficient color development, color change and fading properties, and fastness, and having better texture, the content of the polyester resin is more preferably 1.5 to 4.0% by mass relative to the total amount of the treatment liquid composition in terms of solid content conversion.
[0035] 1.2. Cross-linking agent
[0036] The treatment liquid composition contains a cross-linking agent.
[0037] The treatment liquid composition contains a crosslinking agent to impart crosslinking properties, thereby allowing the polyester resin to bond with the dye and the fabric, thereby obtaining a printed product having sufficient color development, excellent color change and fading resistance, and excellent fastness.
[0038] As a crosslinking agent, it is possible to appropriately select and use from known crosslinking agents, and the crosslinking reaction can be initiated at room temperature or by heating. As such a crosslinking agent, for example, a self-crosslinking crosslinking agent, a compound having multiple functional groups that react with an unsaturated carboxylic acid component in the molecule, and a metal having a multivalent coordination tooth, etc. can be listed.
[0039] From the viewpoint of obtaining a printed material having more adequate color development, color change and fading resistance, and fastness, the cross-linking agent preferably contains an isocyanate group and / or an oxazoline group.
[0040] Examples of the isocyanate group-containing crosslinking agent include water-dispersible (blocked) polyisocyanates, etc. In addition, the (blocked) polyisocyanate refers to a polyisocyanate and / or a blocked polyisocyanate.
[0041] Examples of the water-dispersible polyisocyanate include polyisocyanates obtained by dispersing a polyisocyanate imparted with hydrophilicity by a polyethylene oxide chain in water using an anionic dispersant or a nonionic dispersant.
[0042] Examples of polyisocyanates include diisocyanates such as hexamethylene diisocyanate and isophorone diisocyanate, and derivatives (modified products) of polyisocyanates such as trimethylolpropane adducts, biuret bodies and isocyanurate bodies of these diisocyanates. These polyisocyanates may be used alone or in combination of two or more.
[0043] The water-dispersible blocked polyisocyanate is formed by blocking the isocyanate group of the water-dispersible polyisocyanate with a blocking agent. Examples of the blocking agent include diethyl malonate, ethyl acetoacetate, ε-caprolactam, butanone oxime, cyclohexanone oxime, 1,2,4-triazole, dimethyl-1,2,4-triazole, 3,5-dimethylpyrazole, and imidazole. These blocking agents may be used alone or in combination of two or more.
[0044] As such an isocyanate group-containing crosslinking agent, a commercially available product may be used. Examples of commercially available products include Fixer #100ECO, #104EA, #220, 70ECO, #70, #410, and #400 (the above are trade names, Murayama Chemical Research Institute); Elastron (registered trademark) BN-11, BN-27, BN-69, and BN-77 (the above are trade names, Daiichi Kogyo Seiyaku Co., Ltd.).
[0045] Examples of the cross-linking agent containing an oxazoline group include compounds having two or more oxazoline groups in the molecule. Examples of such oxazoline group-containing compounds include 2,2'-bis(2-oxazoline), 2,2'-methylene-bis(2-oxazoline), 2,2'-ethylene-bis(2-oxazoline), 2,2'-trimethylene-bis(2-oxazoline), 2,2'-tetramethylene-bis(2-oxazoline), 2,2'-hexamethylene-bis(2-oxazoline), 2,2'-octamethylene-bis(2 -oxazoline), 2,2'-ethylene-bis(4,4'-dimethyl-2-oxazoline), 2,2'-p-phenylene-bis(2-oxazoline), 2,2'-m-phenylene-bis(2-oxazoline), 2,2'-m-phenylene-bis(4,4'-dimethyl-2-oxazoline), bis(2-oxazolinylcyclohexane) sulfide, bis(2-oxazolinylnorbornane) sulfide and oxazoline ring-containing polymers. These oxazoline group-containing compounds may be used alone or in combination of two or more.
[0046] The oxazoline group-containing compound is preferably a water-soluble oxazoline group-containing compound because the polyester resin can be more firmly bonded to the dye and the fabric, thereby obtaining a printed or dyed product having even better fastness.
[0047] As such an oxazoline group-containing crosslinking agent, commercially available products may be used, such as Epocros (registered trademark) K-2010, K-2020, K-2030, K-2035E, WS-300, WS-500 and WS-700 (the above are trade names, Nippon Catalyst Co., Ltd.).
[0048] The cross-linking agent may be used alone or in combination of two or more.
[0049] From the viewpoint of obtaining a printed material having more sufficient color development, color change and fading resistance, and fastness, the content of the crosslinking agent is preferably 0.1 to 10.0% by mass in terms of solid content relative to the total amount of the treatment liquid composition.
[0050] From the perspective of obtaining a printed material with more adequate color development, color change and fading properties, and fastness, the preferred mass ratio of polyester resin to crosslinking agent (polyester resin: crosslinking agent) is 1:0.01 to 1:1.2. From the perspective of obtaining a printed material with more adequate color development, color change and fading properties, and fastness, and good texture, the preferred mass ratio of polyester resin to crosslinking agent (polyester resin: crosslinking agent) is 1:0.05 to 1:0.70. In addition, when the polyester resin or crosslinking agent is in the form of an emulsion, the mass ratio is calculated based on the solid content conversion.
[0051] 1.3. Water
[0052] The treatment liquid composition contains water.
[0053] After the treatment liquid composition is attached to the fabric, water evaporates and disperses by drying. Examples of water include pure water such as ion exchange water, ultrafiltration water, and distilled water, and water such as ultrapure water that has ionic impurities removed as much as possible. In addition, water sterilized by ultraviolet irradiation or addition of hydrogen peroxide is preferred because it can inhibit the growth of mold or bacteria when the treatment liquid composition is stored for a long time.
[0054] The water content is 30 to 98% by mass, preferably 35 to 96% by mass, and more preferably 40 to 94% by mass relative to the total amount of the treatment liquid composition. By making the water content within the above range, the increase in the viscosity of the treatment liquid can be suppressed, and the workability when the treatment liquid is attached to the fabric and the drying property after attachment can be improved.
[0055] In order to obtain higher affinity and higher safety for fabrics containing fibers having hydroxyl groups, the treatment liquid composition is preferably an aqueous treatment liquid composition. In addition, in this embodiment, "aqueous" means that the content of water is 30% by mass or more relative to the total amount of the composition.
[0056] 1.4. Other ingredients
[0057] The treatment liquid composition may contain various additives such as a surfactant, a solubilizing agent, a viscosity modifier, a pH modifier, an antioxidant, a preservative, a mildew preventer, a corrosion inhibitor, and a chelating agent.
[0058] The additives may be used alone or in combination of two or more.
[0059] The content of each additive is, for example, approximately 0.01 to 5.0% by mass relative to the total amount of the treatment liquid composition.
[0060] 1.5. Preparation method of treatment liquid composition
[0061] The treatment liquid composition can be prepared by mixing the components in any order and filtering to remove impurities or foreign matter as needed. As a method for mixing the components, a method of sequentially adding the components to a container equipped with a stirring device such as a mechanical stirrer and a magnetic stirrer and stirring and mixing the components can be used. As a filtering method, centrifugal filtration and filter filtration can be listed.
[0062] 1.6. Physical properties of treatment liquid composition
[0063] The physical properties of the treatment liquid composition can be arbitrarily adjusted according to the type of fabric or the method of attaching the treatment liquid composition to the fabric, that is, the coating method, etc. The coating method of the treatment liquid composition will be described later.
[0064] 1.6.1. Viscosity
[0065] The viscosity of the treatment liquid composition at 20° C. is preferably 1.5 to 100 mPa·s. When the viscosity of the treatment liquid is within the above range, the coating properties such as the ease of spreading of the treatment liquid when the treatment liquid is attached to a fabric can be improved.
[0066] The viscosity of the treatment liquid composition can be measured, for example, using a viscoelasticity tester MCR-300 (Pysica). Specifically, the treatment liquid composition can be measured by adjusting the temperature to 20°C and reading the shear viscosity (mPa·s) at a shear rate of 200 (1 / s).
[0067] Surface tension
[0068] The surface tension of the treatment liquid composition at 25°C is preferably 30 to 50 mN / m. By setting the surface tension of the treatment liquid composition at 25°C to the above range, appropriate wettability or permeability to the fabric is exhibited. In addition, since the treatment liquid composition is easily uniformly absorbed by the fabric, the difference in the amount of adhesion generated when the treatment liquid composition is applied, that is, the occurrence of uneven coating, can be suppressed.
[0069] The surface tension of the treatment liquid composition can be measured, for example, using an automatic surface tensiometer CBVP-Z (Kyowa Surface Science Co., Ltd.) Specifically, it can be measured by reading the surface tension of a platinum plate wetted with the treatment liquid composition in an environment of 25°C.
[0070] 2. Inkjet ink composition
[0071] The inkjet ink composition (hereinafter also referred to as "ink composition") is used to print and dye fabric to which the treatment liquid composition of the present embodiment is attached, thereby producing a printed article. Next, the ink composition will be described.
[0072] The ink composition according to the present embodiment contains a disperse dye and water.
[0073] 2.1. Disperse dyes
[0074] In order to obtain excellent color development for the fabric to which the treatment liquid composition is attached, the ink composition contains a disperse dye as a dye. Disperse dyes are usually in the form of particles and are color materials dispersed in a dispersion medium by a dispersant. In addition, disperse dyes are usually nonionic dyes having a hydrophilic group and an appropriate polar group. Disperse dyes can be used alone or in combination of two or more.
[0075] Examples of the disperse dye include CI disperse yellow, CI disperse red, CI disperse blue, CI disperse orange, CI disperse violet, CI disperse green, CI disperse brown, and CI disperse black.
[0076] Among these, sublimation dyes are preferred as dispersants. Here, "sublimation dyes" refer to dyes having a property of sublimating by heating.
[0077] Specific examples of such sublimation dyes include CI Disperse Yellow 3, 7, 8, 23, 39, 51, 54, 60, 71, and 86; CI Disperse Orange 1, 1:1, 5, 20, 25, 25:1, 33, 56, and 76; CI Disperse Brown 2; CI Disperse Red 11, 50, 53, 55, 55:1, 59, 60, 65, 70, 75, 93, 146, 158, 190, 190:1 , 207, 239 and 240; CI Vat Red 41; CI Disperse Violet 8, 17, 23, 27, 28, 29, 36 and 57; CI Disperse Blue 14, 19, 26, 26:1, 35, 55, 56, 58, 64, 64:1, 72, 72:1, 81, 81:1, 91, 95, 108, 131, 141, 145 and 359; CI Solvent Blue 36, 63, 105 and 111, etc.
[0078] In this embodiment, from the viewpoint of obtaining a printed product having better dyeability and sufficient color development for the fabric to which the treatment liquid composition is attached, cyan dye, red dye and yellow dye are preferred. From the viewpoint of obtaining a printed product having further better dyeability and sufficient color development, CI Disperse Blue 359 is more preferred as a cyan dye, CI Disperse Red 60 is more preferred as a red dye, and CI Disperse Yellow 54 is more preferred as a yellow dye.
[0079] From the viewpoint of achieving the effects of the present embodiment more effectively and reliably, the content of the color material is preferably 0.05 to 20% by mass relative to the total amount of the ink composition.
[0080] 2.2. Water
[0081] The ink composition contains water.
[0082] As water, including preferred embodiments, reference may be made to the water contained in the above-mentioned treatment liquid composition.
[0083] From the viewpoint of achieving the effects of the present embodiment more effectively and reliably, the content of water is preferably 30 to 80% by mass relative to the total amount of the ink composition.
[0084] 2.3. Dispersants
[0085] The ink composition may also contain a dispersant.
[0086] When the ink composition contains a dispersant, the dispersibility of the disperse dye is excellent and the ink composition has excellent clogging resistance. Examples of the dispersant include sodium naphthalenesulfonate-formaldehyde condensates and resins. Sodium naphthalenesulfonate-formaldehyde condensates are compounds or salts thereof obtained by condensing a sulfonate having a naphthalene ring in the molecule with formaldehyde. The dispersant may be used alone or in combination of two or more.
[0087] From the perspective of having better dispersibility, it is preferred that the dispersant contain a resin. As the resin, for example, polyurethane resins, styrene acrylic resins, acrylic resins, fluorene resins, polyolefin resins, rosin-modified resins, terpene resins, polyester resins, polyamide resins, epoxy resins, vinyl chloride resins, vinyl chloride-vinyl acetate copolymers, and ethylene vinyl acetate resins can be cited. Among these, from the perspective of excellent clogging resistance, the resin is preferably a polyurethane resin and a styrene acrylic resin, and more preferably a styrene acrylic resin.
[0088] As the polyurethane resin, there is no particular limitation as long as it is a resin having a carbamate bond in the molecule. As the polyurethane resin, there can be cited polyether polyurethane resins containing an ether bond in the main chain in addition to the carbamate bond, polyester polyurethane resins containing an ester bond in the main chain, and polycarbonate polyurethane resins containing a carbonate bond in the main chain. The polyurethane resin can be used alone or in combination of two or more.
[0089] As the polyurethane resin, commercially available products may also be used. Examples of commercially available products include Takelac (registered trademark) W6110 (trade name) manufactured by Mitsui Chemicals, Acrit (registered trademark) WBR-022U (trade name) manufactured by Taisei Fine Chemical, Permarin (registered trademark) UX-368T (trade name), Uprene (registered trademark) UXA-307 (trade name) and U Coat (registered trademark) UWS-145 (trade name) manufactured by Sanyo Chemical Industries, and Solsperse (registered trademark) 47000 (trade name) manufactured by Lubrizol Corporation.
[0090] Examples of the styrene acrylic resin include styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylate copolymers, styrene-α-methylstyrene-acrylic acid copolymers, and styrene-α-methylstyrene-acrylic acid-acrylate copolymers. These copolymers may be in the form of random copolymers, block copolymers, alternating copolymers, and graft copolymers.
[0091] As the styrene acrylic resin, commercially available products may be used, and examples of commercially available products include Joncryl (registered trademark) 67 (trade name) manufactured by BAS Japan Co., Ltd. and Solsperse (registered trademark) 43000 (trade name) manufactured by Lubrizol Corporation.
[0092] From the viewpoint of achieving the effects of the present embodiment more effectively and reliably, the content of the dispersant is preferably 3.0 to 8.0% by mass relative to the total amount of the ink composition.
[0093] Surfactants
[0094] The ink composition may also contain a surfactant.
[0095] Examples of the surfactant include acetylene glycol surfactants, fluorine surfactants, and silicone surfactants. The surfactant may be used alone or in combination of two or more.
[0096] Examples of the acetylene glycol-based surfactant include 2,4,7,9-tetramethyl-5-decyn-4,7-diol and an alkylene oxide adduct thereof, and 2,4-dimethyl-5-decyn-4-ol and an alkylene oxide adduct thereof.
[0097] As the acetylene glycol surfactant, commercial products may also be used. Commercial products include, for example, Olfine (registered trademark) 104 series (trade names) and E series (trade names) manufactured by Nissin Chemical Industry (strain) and Surfynol (registered trademark) series (trade names) manufactured by Air Products and Chemicals Incorporated.
[0098] Examples of the fluorine-based surfactant include perfluoroalkyl sulfonates, perfluoroalkyl carboxylates, perfluoroalkyl phosphates, perfluoroalkyl ethylene oxide adducts, perfluoroalkyl betaines, and perfluoroalkyl amine oxide compounds.
[0099] As the fluorine-based surfactant, a commercially available product may be used. Examples of the commercially available product include S-144 (trade name) and S-145 (trade name) manufactured by Asahi Glass Co., Ltd.
[0100] Examples of the silicone-based surfactant include polysiloxane-based compounds and polyether-modified organosiloxanes.
[0101] As the silicone surfactant, commercially available products may be used, such as BYK (registered trademark) series 306, 307, 333, 341, 345, 346, 347, 348 and 349 (these are trade names) manufactured by BYK Chemical Japan Co., Ltd.
[0102] From the viewpoint of achieving the effects of the present embodiment more effectively and reliably, the content of the surfactant is preferably 0.5 to 5.0% by mass relative to the total amount of the ink composition.
[0103] 2.5. Water-soluble organic solvents
[0104] The ink composition may contain a water-soluble organic solvent.
[0105] Examples of the water-soluble organic solvent include glycerol; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether , propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether and triethylene glycol monomethyl ether; nitrogen-containing solvents such as 2-pyrrolidone, N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, tert-butanol, isobutanol, n-pentanol, 2-pentanol, 3-pentanol and tert-pentanol.
[0106] The water-soluble organic solvent may be used alone or in combination of two or more.
[0107] From the viewpoint of achieving the effects of the present embodiment more effectively and reliably, the content of the water-soluble organic solvent is preferably 5 to 30% by mass relative to the total amount of the ink composition.
[0108] 2.6. Other ingredients
[0109] The ink composition may contain various additives such as a solubilizing agent, a viscosity adjusting agent, a pH adjusting agent, an antioxidant, a preservative, a mildew preventer, a corrosion inhibitor, and a chelating agent for capturing metal ions that affect dispersion.
[0110] The additives may be used alone or in combination of two or more.
[0111] Examples of the preservative include sodium pentachlorophenol, sodium 2-pyridinethiol-1-oxide, and 1,2-dibenzothiazoline-3-one.
[0112] As the preservative, a commercial product may also be used. Commercial products include, for example, CRL, BND, GXL, XL-2 and TN (the above are trade names) of the Proxel (registered trademark) series manufactured by Lonza Japan. The preservative may be used alone or in combination of two or more.
[0113] The content of each additive is about 0.01 to 5.0% by mass based on the total amount of the ink composition.
[0114] 2.7. Method for producing ink composition
[0115] The ink composition can be prepared by mixing disperse dye, water and other components as required in any order, and filtering or the like to remove impurities or foreign matter as required. As a method for mixing the components, a method of sequentially adding the components to a container having a stirring device such as a mechanical stirrer and a magnetic stirrer and stirring and mixing the components can be used. As a filtering method, centrifugal filtration and filter filtration can be cited.
[0116] In addition, in order to disperse the disperse dye more well in the ink composition, a dye dispersant may be prepared in advance, and the ink composition may be prepared using the dye dispersant instead of the disperse dye. The dye dispersant may be obtained by, for example, mixing the disperse dye, water, and the dispersant in any order and dispersing them using a paint disperser or the like.
[0117] 3. Combination group
[0118] The composition set comprises the above-mentioned treatment liquid composition and the above-mentioned ink composition.
[0119] In this embodiment, the treatment liquid composition is attached to a fabric containing fibers having hydroxyl groups in advance to obtain a fabric to which the treatment liquid composition is attached. Then, the fabric to which the treatment liquid composition is attached is printed with an ink composition to easily obtain a printed product having sufficient color development, color change and fading properties over time, and fastness such as resistance to friction.
[0120] 4. Cloth
[0121] The fabric according to the present embodiment includes fibers having a hydroxyl group.
[0122] Examples of fibers having hydroxyl groups include natural fibers such as cotton, linen, wool, and silk; synthetic fibers such as polypropylene, polyester, acetate, triacetate, polyamide, and polyurethane, and fibers having hydroxyl groups in their structures; biodegradable fibers such as polylactic acid, etc. In addition, fibers having hydroxyl groups may be blended fibers of these fibers.
[0123] From the perspective of simply obtaining a printed fabric having more sufficient color development, color change and fading resistance, and fastness, having good texture, and reduced yellowing, cotton is preferred as the fabric.
[0124] As the form of the cloth, for example, textiles, knitwear, nonwoven fabrics, cloth, and clothing and other apparel can be listed. Among the clothing and other apparel, household items such as sewn T-shirts, handkerchiefs, scarves, towels, handbags, cloth bags, curtains, bed sheets, bedspreads and wallpaper can be listed; cloth before and after cutting as a component before sewing. As these forms, a long form wound into a roll, a form cut into a specified size, and a form of a product shape can be listed. In addition, as long as the cloth is attached with a treatment liquid composition, a cloth pre-applied with a treatment liquid composition can also be used as the cloth.
[0125] The basis weight of the cloth is preferably, for example, 1.0 to 10.0 oz. When the basis weight of the cloth is within such a range, recording can be performed well.
[0126] As the fabric, as long as it contains fibers having hydroxyl groups, fabrics pre-colored with dyes can also be used. The treatment liquid composition can suppress the generation of treatment marks on the basis of ensuring the color development, color change and fading resistance and fastness of the fabric, so even pre-colored fabrics can be used as long as they contain fibers having hydroxyl groups. That is, even if the grey fabric is colored, good color development can be achieved, color change and fading resistance and fastness can be maintained, and printing and dyeing that generates treatment marks can be suppressed, so the quality and commodity value of the printed product as a product can be improved compared with the past.
[0127] Examples of dyes for pre-coloring fabrics include water-soluble dyes such as acid dyes and basic dyes, disperse dyes in combination with dispersants, reactive dyes, solvent dyes, etc. When cotton fabrics are used as fabrics, disperse dyes and reactive dyes suitable for dyeing cotton are preferably used, and disperse dyes are more preferred.
[0128] 5. Printing and dyeing methods
[0129] The printing and dyeing method of this embodiment includes a treatment liquid composition attaching step of attaching the treatment liquid composition to a cloth containing fibers having hydroxyl groups. By performing this step, a cloth to which the treatment liquid composition is attached can be obtained. In addition, by attaching the ink composition to the cloth, a printed product having sufficient color development, color change and fading resistance, and fastness can be obtained.
[0130] The printing and dyeing method preferably includes an ink composition attaching step of attaching the ink composition to the fabric to which the treatment liquid composition is attached after the above-mentioned treatment liquid composition attaching step. In addition, the ink composition attached to the fabric is not particularly limited as long as it contains a disperse dye, and for example, the inkjet ink composition involved in this embodiment can be used. In addition, regarding the ink composition attaching step, reference can be made to the printing and dyeing method using the inkjet method described later.
[0131] The printing and dyeing method can be applied to various fabrics and can perform printing well.
[0132] The amount of the treatment liquid composition deposited on the fabric is preferably 0.02 to 0.5 g / cm 2 More preferably, 0.02 to 0.3 g / cm 2 By setting the attached amount of the treatment liquid composition to the above range, the treatment liquid composition can be further uniformly attached to the cloth, the cohesion unevenness of the image in the printed article can be further suppressed, and the color development can be improved.
[0133] As a method for attaching the treatment liquid composition to the fabric, for example, there can be cited an immersion coating method in which the fabric is immersed in the treatment liquid composition, a roll coating method in which the treatment liquid composition is applied using a roll roller or a roll coater, a spray coating method in which the treatment liquid composition is sprayed using a spray device, and an inkjet coating method in which the treatment liquid composition is sprayed using an inkjet method. These coating methods may be used alone to attach the treatment liquid composition to the fabric, or two or more methods may be combined to attach the treatment liquid composition to the fabric.
[0134] In this embodiment, from the perspective of increasing the design freedom of the amount of the treatment liquid composition adhered, being less likely to experience adverse conditions during adhesion, and being able to allow the treatment liquid composition to adhere evenly to the fabric, it is preferred to use rollers such as a rolling roller and a roller coater to allow the treatment liquid composition to adhere to the fabric.
[0135] The dyeing method may include a drying step of the treatment liquid composition after the treatment liquid composition is attached to the fabric. The treatment liquid composition may be dried naturally, but drying with heating is preferred from the viewpoint of increasing the amount of the treatment liquid composition attached to the fabric and increasing the drying speed.
[0136] Examples of the heating method include hot pressing, normal pressure steam, high pressure steam, and thermosetting. Examples of the heat source for heating include infrared rays (lamp).
[0137] In addition, the heating temperature is preferably 180° C. or less, for example. Thus, even if the fabric is pre-dyed with a dye, sublimation of the dye due to heat drying can be suppressed, thereby suppressing fading of the color of the fabric. In addition, the lower limit of the heating temperature is preferably 100° C. or more as long as the medium such as water contained in the treatment liquid composition is volatilized.
[0138] In the printing and dyeing method, after the treatment liquid composition is attached to the fabric, a washing step may be included as necessary. By including this step in the printing and dyeing method, components contained in the treatment liquid composition that are not attached to the fabric can be removed.
[0139] 6. Inkjet printing and dyeing method
[0140] The inkjet printing method is a method of attaching an ink composition to a cloth to which a treatment liquid composition is attached using an inkjet method. By adopting the inkjet method, a dyeing portion with a fine pattern can also be easily and reliably formed. In addition, it can be applied to various cloths and can be printed well. By the inkjet printing method, even for a thick grey cloth, the color difference between the front and back can be small and printed well. As the inkjet printing method, for example, an indirect printing recording method and a direct printing recording method can be cited.
[0141] 6.1. Inkjet recording device
[0142] As an inkjet recording device for a printing and dyeing method, there is no particular limitation as long as it can have at least an ink container for containing an ink composition and a recording head connected thereto, and eject the ink composition from the recording head to form an image on a cloth to which a treatment liquid composition is attached or a transfer paper as an intermediate transfer medium. In addition, as an inkjet recording device, any of a serial type and a line type can be used. In these types of inkjet recording devices, a recording head is mounted, and while the relative positional relationship between the cloth or transfer paper and the recording head is changed, droplets of the ink composition are ejected from the nozzle hole of the recording head at a specified timing in an intermittent and specified volume manner. In this way, the ink composition can be attached to the cloth or transfer paper to form a specified transfer image.
[0143] Generally, in a serial inkjet recording device, the conveying direction of the recording medium intersects with the direction of the reciprocating motion of the recording head, and the relative positional relationship between the recording medium and the recording head changes by the combination of the reciprocating motion of the recording head and the conveying motion of the recording medium. In addition, in this case, a plurality of nozzle holes are generally arranged on the recording head, and a row of nozzle holes, i.e., a nozzle row, is formed along the conveying direction of the recording medium. In addition, sometimes, a plurality of nozzle rows are formed on the recording head depending on the type or amount of the ink composition.
[0144] In addition, in a line-type inkjet recording device, the recording head does not reciprocate, but the relative positional relationship between the recording medium and the recording head is changed by the conveyance of the recording medium, thereby changing the relative positional relationship between the recording medium and the recording head. In this case, a plurality of nozzle holes are usually arranged on the recording head, and a nozzle row is formed along a direction intersecting the conveyance direction of the recording medium.
[0145] 6.2. Indirect printing and dyeing recording method
[0146] The inkjet printing method of the present embodiment includes: a treatment liquid composition attachment step, in which the treatment liquid composition is attached to a fabric containing fibers having hydroxyl groups; a discharge step, in which the ink composition is discharged from a recording head and attached to an intermediate transfer medium; and a transfer step, in which the ink composition attached to the intermediate transfer medium is transferred to the fabric attached with the treatment liquid composition obtained by the treatment liquid composition attachment step. Specifically, in the printing method, an ink composition containing disperse dyes such as sublimation dyes is discharged using a liquid jet head as a recording head and attached to an intermediate transfer medium, and the surface of the intermediate transfer medium to which the ink composition is attached is heated in a state where the surface of the fabric to which the treatment liquid composition is attached faces each other, thereby transferring the disperse dyes contained in the ink composition to the fabric to which the treatment liquid composition is attached. In the present embodiment, such a printing method is also referred to as an indirect printing recording method. According to the printing method, printing can be performed well without limiting the form of the fabric.
[0147] 6.2.1. Treatment liquid composition attachment step
[0148] Regarding the treatment liquid composition attaching step, the above-mentioned printing and dyeing method can be referred to.
[0149] 6.2.2. Spraying process
[0150] In the ejection step, the heated ink composition is ejected from the liquid ejection head and attached to the intermediate transfer medium. Specifically, the pressure generating mechanism is driven to eject the ink composition filled in the pressure generating chamber of the liquid ejection head from the nozzle.
[0151] As the intermediate transfer medium, for example, paper such as plain paper and recording medium provided with an ink receiving layer can be used. The above-mentioned recording medium provided with an ink receiving layer is called, for example, special paper for inkjet and coated paper. Among these, paper provided with an ink receiving layer containing inorganic particles such as silicon dioxide is more preferably provided. Thus, in the process of drying the ink composition imparted to the intermediate transfer medium, an intermediate record material that has suppressed bleeding to the recording surface can be obtained. In addition, if it is such a medium, it is easier to retain disperse dyes on the surface of the recording surface, and in the subsequent transfer process, the sublimation of disperse dyes can be carried out more effectively.
[0152] In this step, multiple ink compositions may be used. This can, for example, make the color range that can be expressed wider. One of the multiple ink compositions may be the ink composition of this embodiment, or two or more of the multiple ink compositions may be the ink composition of this embodiment.
[0153] 6.2.3. Transfer process
[0154] The transfer step is a step of heating the intermediate transfer medium in a state where the surface of the intermediate transfer medium to which the ink composition is attached is placed opposite to the surface of the fabric to which the treatment liquid composition is attached, thereby transferring the disperse dye contained in the ink composition to the fabric to which the treatment liquid composition is attached. Thus, a printed article is obtained which is a fabric to which the disperse dye is transferred and to which the ink composition is attached.
[0155] In this step, the intermediate transfer medium to which the ink composition is applied and the cloth to which the treatment liquid composition is attached may be heated while being placed facing each other. In this step, it is more preferable to heat the intermediate transfer medium while being placed in close contact with the cloth to which the treatment liquid composition is attached. Thus, for example, a more vivid image can be recorded, i.e., dyed, on the cloth to which the treatment liquid composition is attached.
[0156] Examples of the heating method include steam heating using steam, hot pressing using dry heat, hot melt, HT steam heating using superheated steam, and HP steam heating using pressurized steam. The fabric to which the ink composition has been applied may be subjected to the heating treatment immediately or after a predetermined period of time. Dry heating is preferred as the heating method in order to obtain a printed material having sufficient color development, color change and fading resistance, and fastness.
[0157] The heating temperature is preferably 160 to 220° C., more preferably 190 to 210° C. By setting the heating temperature within the above range, the energy required for transfer can be further reduced, and the productivity of printed materials tends to be more excellent. In addition, the color development of printed materials tends to be more excellent.
[0158] The heating time varies depending on the heating temperature, and is preferably 30 to 120 seconds, and more preferably 40 to 90 seconds. By making the heating time within the above range, the energy required for transfer can be further reduced, and the productivity of the printed material tends to be more excellent. In addition, the color development of the printed material tends to be more excellent.
[0159] The amount of the ink composition deposited on the fabric by transfer is preferably 1.5 to 6.0 mg / cm per unit area of the fabric. 2 By setting the amount of the ink composition to be applied within the above range, the color development of an image or the like formed by printing and dyeing can be improved, and the drying of the ink applied to the fabric can be ensured, thereby reducing the bleeding of the image or the like.
[0160] 6.2.4. Other processes
[0161] This method may include an intermediate treatment step and a post-treatment step as necessary.
[0162] As an intermediate treatment step, for example, there is a step of preheating the fabric to which the treatment liquid composition is attached.
[0163] As the post-treatment step, for example, there is a step of washing the printed material.
[0164] 6.2. Direct printing and dyeing recording method
[0165] The inkjet printing method may further include: a treatment liquid composition attachment step, in which the treatment liquid composition is attached to a fabric containing fibers having hydroxyl groups; and an ink composition attachment step, in which the ink composition is ejected from a recording head and the ink composition is attached to the fabric attached with the treatment liquid composition obtained by the treatment liquid composition attachment step. In the present embodiment, such a printing method is also referred to as a direct printing recording method. According to the printing method, a dyeing portion of a fine pattern can also be easily and reliably formed. In addition, since there is no need to use a plate such as an intermediate transfer medium, it is excellent in on-demand performance and can appropriately cope with small-volume production and multi-variety production.
[0166] 6.2.1. Step of obtaining a fabric having a treatment liquid composition attached thereto
[0167] Regarding the treatment liquid composition attaching step, the above-mentioned printing and dyeing method can be referred to.
[0168] 6.2.2. Ink composition attachment step
[0169] In the ink composition attaching step, the ink composition is attached to the fabric to which the treatment liquid composition is attached. In addition, the ink composition attaching step may further include a step of attaching an ink composition to the region to which the ink composition is attached.
[0170] In the ink composition adhesion step, the maximum adhesion amount to the fabric is preferably 50 to 200 mg / cm 2 , more preferably 80 to 150 mg / cm 2 When the maximum adhesion amount is within the above range, the color development becomes better. In addition, the friction fastness of the image becomes excellent, and there is a tendency that the aggregation unevenness is not significant.
[0171] In this step, when the ink composition is attached to the cloth to which the treatment liquid composition is attached, it is preferably heated. This allows, for example, recording, that is, dyeing, a clearer image on the cloth to which the treatment liquid composition is attached.
[0172] Examples of the heating method include hot pressing, normal pressure steam, high pressure steam and thermosetting. Examples of the heat source include hot air, infrared rays and microwaves.
[0173] During heating, the surface temperature of the heated fabric is preferably 60 to 180° C. By keeping the surface temperature within the above range, damage to the inkjet head or fabric can be reduced, and the ink can easily wet and spread to the fabric evenly, making it easy to penetrate. In addition, the surface temperature can be measured using a non-contact thermometer (trade name "IT2-80", manufactured by KEYENCE Co., Ltd.), for example.
[0174] The heating time is preferably, for example, 5 seconds or more and 5 minutes or less. By setting the heating time to be within the above range, damage to the inkjet head or the cloth can be reduced, and the cloth can be heated sufficiently.
[0175] 6.2.3. Other processes
[0176] In this method, an intermediate treatment step and a post-treatment step may be included as necessary. For these steps, reference may be made to other steps in the above-mentioned indirect dyeing and printing recording method.
[0177] Example
[0178] Hereinafter, the present invention will be described in more detail using Examples and Comparative Examples. The present invention is not limited to the following Examples at all.
[0179] 1. Preparation of treatment liquid composition for dye printing
[0180] (Examples 1 to 15 and Comparative Examples 1 to 14)
[0181] According to the compositions described in Tables 1 and 2, the components were added to a mixing tank, mixed and stirred, and further filtered through a 5 μm membrane filter to obtain treatment liquid compositions.
[0182] In addition, the numerical values of the compounding amounts of each component in Tables 1 and 2 represent mass %. The "solid content" in the resin and the crosslinking agent represents mass %. The "Tg" in the resin represents the glass transition temperature (°C). The "resin solid content" represents the solid content (mass parts) of the resin in the treatment liquid composition. The "crosslinking agent solid content" represents the solid content (mass parts) of the crosslinking agent in the treatment liquid composition, and the "crosslinking agent solid content / resin solid content ratio" represents the mass ratio of the polyester resin to the crosslinking agent calculated in terms of solid content conversion.
[0183] In addition, each component shown in Tables 1 and 2 is as follows.
[0184] 〔Resin〕
[0185] (Styrene acrylic resin)
[0186] 6960: Mowinyl (registered trademark) 6960 (trade name, Japan Coating Resin Co., Ltd.)
[0187] (Sulfonic acid group-containing polyester resin)
[0188] · Z-3310: Plascoat (registered trademark) Z-3310 (trade name, Huying Chemical Industry Co., Ltd.)
[0189] ·Z-880: Plascoat (registered trademark) Z-880 (trade name, Huying Chemical Industry Co., Ltd.)
[0190] ·Z-592: Plascoat (registered trademark) Z-592 (trade name, Huying Chemical Industry Co., Ltd.)
[0191] ·Z-687: Plascoat (registered trademark) Z-687 (trade name, Huying Chemical Industry Co., Ltd.)
[0192] · RZ-570: Plascoat (registered trademark) RZ-570 (trade name, Huying Chemical Industry Co., Ltd.)
[0193] (Carboxyl-containing polyester resin)
[0194] · RZ-760: Plascoat (registered trademark) RZ-760 (trade name, Huying Chemical Industry Co., Ltd.)
[0195] (Polyester resin)
[0196] MD-1480: Vylonal (registered trademark) MD-1480 (trade name, Toyobo Co., Ltd.)
[0197] MD-2000: Vylonal (registered trademark) MD-2000 (trade name, Toyobo Co., Ltd.)
[0198] 〔Cross-linking agent〕
[0199] ·#220: Fixer#220 (trade name, Murayama Chemical Laboratory Co., Ltd.)
[0200] ·K-2035E: Epocros (registered trademark) K-2035E (trade name, Japan Catalyst Co., Ltd.)
[0201] [Table 1]
[0202]
[0203] [Table 2]
[0204]
[0205] Furthermore, in Comparative Examples 1 and 2, no treatment liquid composition was prepared.
[0206] 2. Preparation of inkjet ink composition
[0207] (Dye dispersant 1~3)
[0208] According to the composition described in Table 3, each component was added to a mixing pot and dispersed using a paint disperser with 0.3 mm zirconia beads to obtain dye dispersants 1 to 3. The numerical values of each component in Table 3 represent mass %.
[0209] In addition, each component shown in Table 3 is as follows.
[0210] 〔Disperse dyes〕
[0211] Disperse Blue 359: CI Disperse Blue 359 (commercially available)
[0212] Disperse Red 60: CI Disperse Red 60 (commercially available)
[0213] Disperse Yellow 54: CI Disperse Yellow 54 (commercially available)
[0214] 〔Dispersant〕
[0215] Solsperse(R)43000: Solsperse(registered trademark)43000 (trade name, acrylic-styrene resin, manufactured by Lubrizol Corporation)
[0216] [Table 3]
[0217]
[0218] (C ink, M ink and Y ink)
[0219] According to the composition listed in Table 4, each component was added to a mixing tank and mixed and stirred for 2 hours using a stirrer. Then, the mixture was filtered using a membrane filter with a pore size of 1 μm, thereby obtaining ink compositions C ink, M ink, and Y ink, respectively. In addition, the numerical values of each component in Table 4 represent mass %.
[0220] In addition, each component shown in Table 4 is as follows.
[0221] 〔Dye dispersant〕
[0222] The dye dispersants 1 to 3 obtained above were used respectively.
[0223] 〔Surfactant〕
[0224] BYK(R)-348: BYK(registered trademark)-348 (trade name, silicone surfactant, manufactured by BYK-Chemical Japan Co., Ltd.)
[0225] 〔Water-soluble organic solvent〕
[0226] ·glycerin
[0227] Propylene glycol
[0228] 〔preservative〕
[0229] · Proxel(R)XL-2: Proxel(registered trademark)XL-2 (trade name, manufactured by Lonza Japan)
[0230] [Table 4]
[0231]
[0232] 3. Production of printed materials
[0233] 3.1. Preparation of fabric with treatment liquid composition attached thereto
[0234] (Examples 1 to 15 and Comparative Examples 3 to 12)
[0235] The treatment liquid compositions of Examples 1 to 15 and Comparative Examples 3 to 12 were used to attach the treatment liquid compositions to fabrics. Specifically, fabrics to which the treatment liquid compositions were attached were obtained by the following operation.
[0236] The treatment liquid composition was impregnated into a white cotton sheet #4000 (trade name, manufactured by Toyobo Co., Ltd.) as a fabric, and the treatment liquid composition was applied to the fabric using a rolling roller in a manner of a rolling ratio of 80%. Then, it was dried at 120° C. for 2 minutes and then further dried at 170° C. for 1 minute to obtain fabrics to which the treatment liquid composition was attached.
[0237] In addition, the rolling rate (S) is calculated by the following formula (1).
[0238] S(%)=[(AB) / B]×100···(1)
[0239] In the formula (1), S represents the rolling ratio (%), A represents the mass of the fabric to which the treatment liquid composition is attached, and B represents the mass of the fabric before the treatment liquid composition is attached.
[0240] (Examples 16 to 20 and Comparative Examples 13 and 14)
[0241] The treatment liquid compositions of Examples 7, 15, 9, 11, 12 and Comparative Examples 13 and 14 were respectively used to attach the treatment liquid compositions to the fabric. Specifically, the fabric to which the treatment liquid compositions were attached was obtained by the following operation.
[0242] The treatment liquid composition was uniformly applied to one side of the chest area of a commercially available T-shirt as a fabric in A4 size by spraying, and then dried at 120°C for 2 minutes and further at 170°C for 30 seconds to obtain fabrics to which the treatment liquid composition was applied.
[0243] 3.2. Preparation of intermediate recording medium with ink composition attached thereto
[0244] (Examples 1 to 20 and Comparative Examples 1 to 14)
[0245] The C ink, M ink, and Y ink were filled into the ink cartridges of the inkjet printer PX-G930 (trade name, manufactured by Seiko Epson Corporation). Then, the ink ejection amount was 12 mg / inch at a resolution of 720 dpi × 720 dpi and a duty ratio of 100%. 2 Under the conditions of , the three inks were attached to the coated surface of the coated paper (TRANSJET Sportline 1254 (trade name), manufactured by Chem Paper) as the intermediate transfer medium in a non-overlapping manner, forming an image with three filled patterns. Thus, an intermediate recording medium with the ink composition attached was obtained.
[0246] 3.3. Printing and dyeing
[0247] (Examples 1 to 15 and Comparative Examples 3 to 12)
[0248] A heat press TP-608M (trade name, manufactured by Taiyo Seiki Co., Ltd.) was used at a temperature of 200°C and a pressure of 4.2 N / cm 3 and 60 seconds, the surface formed by the image of the intermediate recording medium attached with the ink composition obtained above was thermally transferred to the cloth (cotton sheet) attached with the processing liquid composition obtained above, and cloths, i.e., printed materials, attached with C ink, M ink and Y ink were obtained respectively.
[0249] (Examples 16 to 20 and Comparative Examples 13 and 14)
[0250] A heat press TP-608M (trade name, manufactured by Taiyo Seiki Co., Ltd.) was used at a temperature of 200°C and a pressure of 4.2 N / cm 3and 60 seconds, the surface formed by the image of the intermediate recording medium attached with the ink composition obtained above was thermally transferred to the cloth (T-shirt) attached with the processing liquid composition obtained above, and the cloth, i.e., printed matter, attached with C ink, M ink and Y ink was obtained respectively.
[0251] (Comparative Example 1)
[0252] A heat press TP-608M (trade name, manufactured by Taiyo Seiki Co., Ltd.) was used at a temperature of 200°C and a pressure of 4.2 N / cm 3 and 60 seconds, the surface formed by the image of the intermediate recording medium attached with the ink composition obtained above was thermally transferred to a white polyester cloth Carl Dry K-1 (trade name, Toray Industries, Ltd.), thereby obtaining cloths, i.e., printed articles, attached with C ink, M ink, and Y ink, respectively.
[0253] (Comparative Example 2)
[0254] A heat press TP-608M (trade name, manufactured by Taiyo Seiki Co., Ltd.) was used at a temperature of 200°C and a pressure of 4.2 N / cm 3 The surface formed by the image of the intermediate recording medium with the ink composition attached thereto was thermally transferred to a white cotton sheet #4000 (trade name, Nisshinbo Holdings Inc.) for 10 minutes at 37°C and 60 seconds to obtain cloths, i.e., printed articles, with C ink, M ink, and Y ink attached thereto, respectively.
[0255] 4. Evaluation Method
[0256] 4.1. Discoloration and fading
[0257] Using a fluorescence spectrophotometer FD-7 (trade name, manufactured by Konica Minolta Co., Ltd.), the color density (OD value) of the printed matter with C ink, M ink, and Y ink attached just after printing was measured under the following measurement conditions and at a room temperature of 25° C. Then, the printed matter was left at a room temperature of 25° C. for three days, and the color density (OD value) of the printed matter after leaving was measured under the same conditions.
[0258] (Measurement conditions)
[0259] Observation light source: D65
[0260] Observation field: 2°
[0261] Status: T
[0262] UV filter: installation
[0263] The OD value of the printed material immediately after printing was compared with the OD value of the printed material after being left for three days, and the discoloration and fading properties of the printed materials of Examples 1 to 15 and Comparative Examples 1 to 12 were evaluated according to the following evaluation criteria. The results are shown in Tables 5 and 6.
[0264] (Evaluation Criteria)
[0265] A: The decrease rates of the OD values of the three colors are all less than 2%.
[0266] B: The decrease rate of the OD value of any one of the three colors is 2% or more and less than 5%. In addition, the decrease rate of the OD value of the other colors is less than 2%.
[0267] C: The decrease rate of the OD value of any one of the three colors is 5% or more. In addition, the decrease rate of the other OD values is less than 5%.
[0268] 4.2. Color rendering
[0269] 4.2.1. Color development of C ink
[0270] The printed matter with C ink, M ink and Y ink attached was left for three days at a room temperature of 25° C. Then, the color density (OD value) of the printed matter with respect to C ink was measured using a fluorescence spectrophotometer FD-7 (trade name, manufactured by Konica Minolta Co., Ltd.) under the following measurement conditions and at a room temperature of 25° C.
[0271] (Measurement conditions)
[0272] Observation light source: D65
[0273] Observation field: 2°
[0274] Status: T
[0275] UV filter: installation
[0276] Then, the OD values of the printed articles of Examples 1 to 15 and Comparative Examples 1 and 3 to 12 were compared with the OD value of the printed article of Comparative Example 2, and the color development properties of the ink C were evaluated according to the following evaluation criteria. The results are shown in Tables 5 and 6.
[0277] (Evaluation Criteria)
[0278] A: The OD value is 200% or more compared to the OD value of the printed article of Comparative Example 2.
[0279] B: The OD value is 180% or more and less than 200% of the OD value of the printed article of Comparative Example 2.
[0280] C: The OD value is 170% or more and less than 180% of the OD value of the printed article of Comparative Example 2.
[0281] D: The OD value is 160% or more and less than 170% of the OD value of the printed article of Comparative Example 2.
[0282] E: The OD value is less than 160% compared with the OD value of the printed article of Comparative Example 2.
[0283] 4.2.2. Color development of M ink
[0284] The color density (OD value) of the M ink on the printed material after leaving it for three days was measured using a fluorescence spectrophotometer FD-7 (trade name, manufactured by Konica Minolta Co., Ltd.) under the same measurement conditions as above.
[0285] Then, the OD values of the printed articles of Examples 1 to 15 and Comparative Examples 1 and 3 to 12 were compared with the OD value of the printed article of Comparative Example 2, and the color development properties of the M ink were evaluated according to the following evaluation criteria. The results are shown in Tables 5 and 6.
[0286] (Evaluation Criteria)
[0287] A: The OD value is 190% or more compared to the OD value of the printed article of Comparative Example 2.
[0288] B: The OD value is 180% or more and less than 190% of the OD value of the printed article of Comparative Example 2.
[0289] C: The OD value is 170% or more and less than 180% of the OD value of the printed article of Comparative Example 2.
[0290] D: The OD value is 160% or more and less than 170% of the OD value of the printed article of Comparative Example 2.
[0291] E: The OD value is less than 160% compared with the OD value of the printed article of Comparative Example 2.
[0292] 4.2.3. Color rendering of Y ink
[0293] The color density (OD value) of the printed matter to the Y ink after being left for three days was measured using a fluorescence spectrophotometer FD-7 (trade name, manufactured by Konica Minolta Co., Ltd.) under the same measurement conditions as above.
[0294] Then, the OD values of the printed articles of Examples 1 to 15 and Comparative Examples 1 and 3 to 12 were compared with the OD value of the printed article of Comparative Example 2, and the color development properties for the Y ink were evaluated according to the following evaluation criteria. The results are shown in Tables 5 and 6.
[0295] (Evaluation Criteria)
[0296] A: The OD value is 200% or more compared to the OD value of the printed article of Comparative Example 2.
[0297] B: The OD value is 180% or more and less than 200% of the OD value of the printed article of Comparative Example 2.
[0298] C: The OD value is 170% or more and less than 180% of the OD value of the printed article of Comparative Example 2.
[0299] D: The OD value is 160% or more and less than 170% of the OD value of the printed article of Comparative Example 2.
[0300] E: The OD value is less than 160% compared with the OD value of the printed article of Comparative Example 2.
[0301] 4.3. Durability
[0302] After making a printed article with C ink, M ink and Y ink attached according to the above-mentioned printing method, it was placed at room temperature of 25°C for 1 hour. Then, for the recording surface of the printed article, the test was carried out according to the ISO-105X12 wet test, using the Gakushin friction fastness tester AB-301 (trade name, manufactured by TESTER SANGYO CO,.LTD.), and the friction fastness was evaluated using the pollution gray scale according to the following evaluation criteria. The evaluation results represent the excellence of fastness in the order of AA, A, B and C. When the evaluation result is B or above, the fastness can be called excellent. These results are shown in Tables 5 and 6.
[0303] (Evaluation Criteria)
[0304] AA: The friction fastness of the three colors all exceeded level three.
[0305] A: The friction fastness of any one of the three colors is level 3. In addition, the friction fastness of the other colors exceeds level 3.
[0306] B: The friction fastness of any one of the three colors is level 2 or higher and less than level 3. In addition, the friction fastness of the other colors exceeds level 3.
[0307] C: The friction fastness of any one of the three colors is less than level 2. In addition, the friction fastness of the other colors exceeds level 2.
[0308] 4.4. Texture
[0309] After producing printed articles with C ink, M ink, and Y ink attached thereto according to the above-mentioned production of printed articles, the texture of the obtained printed articles was evaluated by sensory tests. Specifically, for the obtained printed articles, five arbitrary judges evaluated them as "not inferior to the original touch of the cloth" or "the printed article became hard and the original touch of the cloth was damaged", and the texture was evaluated according to the results and the following evaluation criteria. When the evaluation result is B or above, the texture can be called excellent.
[0310] A: Four or more judges answered that the texture is “not inferior to the original texture of the fabric”.
[0311] B: Three judges answered that the texture was “not inferior to the original texture of the fabric”.
[0312] C: One or two judges answered “Not inferior to the original texture of the fabric”.
[0313] These results are shown in Table 7. In addition, the description of numerical values and the like in Table 7 is the same as that in Tables 1 and 2.
[0314] [Table 5]
[0315]
[0316] [Table 6]
[0317]
[0318] [Table 7]
[0319]
[0320] As shown in Tables 5 and 6, it can be seen that by allowing the treatment liquid composition of the present embodiment to adhere to cotton fabric containing fibers having hydroxyl groups and printing and dyeing the cotton fabric to which the treatment liquid composition is attached, it is possible to simply obtain a printed fabric having sufficient color development, color change and fading resistance over time, and abrasion resistance.
[0321] In addition, as shown in Table 5, it can be seen that when the mass ratio of polyester resin to crosslinking agent (polyester resin: crosslinking agent) is in the range of 1:0.01 to 1:1.2, printed materials with more sufficient color development, color change and fading properties and fastness can be obtained.
[0322] According to the comparison between Examples 1, 3, 6 and 8 and Examples 2, 4, 5, 7 and 9 to 12, it can be seen that when the content of the polyester resin is in the range of 1.5 to 8.0 mass % calculated as solid content relative to the total amount of the treatment liquid composition, a printed material with more sufficient color development and color change and fading properties and further excellent fastness can be obtained.
[0323] According to the comparison between Examples 7, 9, 11 and 15 to 19 and Examples 12, 20 and Comparative Examples 13 and 14, it can be seen that when the content of the polyester resin is in the range of 1.0 to 6.0 mass % calculated as solid content relative to the total amount of the treatment liquid composition, a printed material with more sufficient color development, color change and fading resistance, and fastness, as well as good texture can be obtained.
[0324] In addition, according to the comparison between Examples 7, 9, 11 and 15 to 19 and Examples 12 and 20, it can be seen that when the mass ratio of polyester resin to cross-linking agent (polyester resin: cross-linking agent) is in the range of 1:0.05 to 1:0.70, a printed material with more sufficient color development, color change and fading resistance, and fastness, and good texture can be obtained.
[0325] According to the comparison between Examples 7, 9, 16 and 18 and Examples 11, 12, 15, 17, 19, 20 and Comparative Examples 13 and 14, it can be seen that when the content of the polyester resin is in the range of 1.5 to 4.0% by mass calculated as solid content relative to the total amount of the treatment liquid composition, a printed material with sufficient color development, color change and fading resistance, and fastness, and further good texture can be obtained.
Claims
1. A composition set, characterized in that: A dye printing treatment liquid composition and an inkjet ink composition are provided. The inkjet ink composition contains disperse dye and water, The dye printing treatment liquid composition is a treatment liquid composition used by attaching to fabrics. The dye printing and dyeing treatment liquid composition contains: Polyester resin with a glass transition temperature of 40°C or above; a cross-linking agent; and water, The fabric includes fibers having hydroxyl groups.
2. The composition set according to claim 1, characterized in that: The content of the polyester resin is 0.5 to 12.5% by mass in terms of solid content relative to the total amount of the treatment liquid composition.
3. The composition set according to claim 1 or 2, characterized in that: The polyester resin contains at least one selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfonic acid group, and sodium salts thereof.
4. The composition set according to claim 1, characterized in that: The cross-linking agent contains at least one group selected from the group consisting of an isocyanate group and an oxazoline group.
5. The composition set according to claim 1, characterized in that: The mass ratio of the polyester resin to the cross-linking agent, that is, the polyester resin: the cross-linking agent, is 1:0.05 to 1:0.
70.
6. An inkjet printing method, characterized in that: include: a treatment liquid composition attaching step of attaching the dye printing treatment liquid composition in the composition group according to any one of claims 1 to 5 to the fabric; A discharge step of discharging the inkjet ink composition in any one of claims 1 to 5 from a recording head and causing it to adhere to an intermediate transfer medium; as well as The transfer step is to transfer the inkjet ink composition attached to the intermediate transfer medium to the fabric to which the dye printing treatment liquid composition is attached obtained in the treatment liquid composition attachment step.
Citation Information
Patent Citations
Polyester fabric for ink-jet printing and pretreatment agent for obtaining the same
JP2009249773A
Ink for inkjet printing and inkjet printing method, and method for manufacturing ink for inkjet printing
JP2019182941A
Textile treatment for sublimation ink transfers
US20170260690A1