Composite electrode for sintering, preparation process, sintering device and sintering method
By using the self-heating carbon material of composite electrodes to generate Joule heat during flash burning of metal and metal-based composite materials, the densification problem caused by small powder resistance is solved, and rapid sintering and efficient preparation of large pieces of materials are achieved.
Patent Information
- Application Number
- CN202211484305.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-24
AI Technical Summary
In the prior art, due to the small resistance of the powder during flash burning of metal and metal-based composite materials, sufficient Joule heat cannot be generated, making it difficult to achieve rapid densification of the material, and large samples cannot be found in the prior art. High power pulsed power supply to provide the necessary energy density.
Using composite electrodes, including refractory high entropy alloys, carbon materials and refractory pure metals, uses conductive silver paste to stimulate the self-heating carbon material in the composite electrode to generate Joule heat, and conduct heat to powder to achieve rapid sintering.
Complete densification of metal or metal-based composite materials in a short time reduces the power requirements for pulsed power devices, and is able to process large samples, improving preparation efficiency and density.
Smart Images

Figure CN115740442B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a composite electrode for sintering, a preparation process, a sintering device and a sintering method. Background Art
[0002] Powder metallurgy is a technology that uses powder as raw material, through forming and sintering, to manufacture metal materials, ceramic materials and various composite materials. It plays an important role in the development of new materials. At present, the powder metallurgy industry mainly uses traditional sintering technology, that is, the powder is molded and placed in a high-temperature furnace for long-term sintering. For example: the traditional sintering of copper-tungsten electrical contact composite materials requires more than 20 hours; the sintering of tungsten carbide cobalt carbide tools requires 40 hours or even longer to achieve densification. The traditional sintering method is not only difficult to obtain high-quality sintered materials, but also long-term high-temperature sintering means huge energy consumption and carbon emissions. However, in the case of tight energy supply, high electricity bills and insufficient electricity supply have brought tremendous pressure to traditional sintering companies.
[0003] In order to overcome the limitations of the traditional sintering method, such as long time, high energy consumption and low quality, the flash sintering method has emerged. The patents applied for by Professor Raj and his colleagues (US9334194B2, US8940220B2) describe in detail the connotation, operation method and related equipment of flash sintering of materials, but the flash sintering method is only effective for ceramic materials; the patent (CN110577399B) reports a multi-field coupled flash sintering system based on induction heating, providing a non-traditional new flash sintering technology based on induction heating, short process and multi-field coupling, but this invention uses powder heating and induction heating to achieve flash burning of samples. When the sample is large, a very high power output is required to meet the flash burning conditions of metal powders; the patent (CN113523273B) reports a powder metallurgy method for rapidly preparing ultrafine-grained pure tungsten materials under multi-field coupling. This invention only needs to loosely load metal tungsten powder into the powder metallurgy mold, and then directly perform multi-field coupled rapid sintering at room temperature. Pure tungsten metal material close to the theoretical density can be successfully prepared within 1 to 20 minutes. This method only uses the Joule heat of the powder during the sintering process to generate heat, so even if it is sintered for a long time at a very large current, it cannot fully achieve densification. At present, the existing flash burning technology is based on the Joule heat of the powder itself to achieve the flash burning of the powder blank. However, when the powder is a metal powder, the resistance of the metal powder is small, and the Joule heat effect is not obvious. Only under a very large current can sufficient Joule heat be generated to achieve material flash burning. This feature leads to the high power requirements of the flash burning pulse power supply for traditional flash burning; and when the size of the flash burning sample is too large, it is impossible to find a pulse power supply with a high enough power to provide sufficient energy density to achieve flash burning densification of large samples.
[0004] Flash sintering of metals and metal-based composite materials has many advantages such as short time, high efficiency, energy saving and greenness. In the flash sintering process of metals and metal-based composite materials, there must be a thermal runaway process to achieve rapid densification of the material, that is, the powder must obtain enough energy in a short time to achieve a sharp rise in temperature. When the resistance of the metal powder is small, the Joule heat effect is not obvious, and often it cannot generate enough heat to achieve flash sintering under a large current. This requires the pulse power supply device to have extremely high power, that is, a large output current, in order to provide enough heat for the powder to achieve flash sintering. However, high-power pulse power supply devices not only have harsh manufacturing technology and high manufacturing costs, but also the pulse power supply devices under the existing technology cannot provide enough energy for the flash sintering of large pieces of metal and metal-based composite materials. Therefore, there is a problem that due to the small resistance during the flash sintering of metals and metal-based composite materials, it is impossible to generate enough Joule heat to make the material flash densified. Summary of the invention
[0005] In order to overcome the problems existing in the prior art, the present invention provides a composite electrode for sintering, a preparation process, a sintering device and a sintering method to solve the above problems existing in the prior art.
[0006] A method for preparing a composite electrode for sintering comprises the following steps:
[0007] (1) Cut refractory high entropy alloys, carbon materials and refractory pure metals into required shapes;
[0008] (2) Applying conductive silver paste on the contact interface between refractory high entropy alloy and carbon material and the contact interface between carbon material and refractory pure metal;
[0009] (3) The refractory high entropy alloy and the refractory pure metal are arranged at the two ends, and the carbon material is arranged in the middle. After the three materials are stacked together, they are placed in a drying oven and baked at a certain temperature for a period of time to obtain a composite electrode.
[0010] The present invention also provides a composite electrode for sintering, wherein the composite electrode is obtained by the preparation method of the present invention, and comprises: a refractory high entropy alloy, a carbon material and a refractory pure metal, wherein:
[0011] Wherein, the refractory high entropy alloy is arranged at the upper end of the composite electrode, and its length accounts for 50-80% of the entire composite electrode;
[0012] The carbon material is arranged in the middle of the composite electrode, and its length accounts for 15-30% of the entire composite electrode;
[0013] The refractory pure metal is arranged at the lower end of the composite electrode, and its length accounts for 5-20% of the entire composite electrode.
[0014] According to the aspects described above and any possible implementation method, an implementation method is further provided, wherein the material of the refractory high entropy alloy is one of NbMoTaW, AlNbTiV, and TaNbTiV; the material of the carbon material is one of graphite paper, graphite block, and graphite felt; the material of the refractory pure metal is one of pure tungsten, pure tantalum, and pure rhenium.
[0015] According to the aspects and any possible implementations described above, an implementation is further provided, in which a conductive silver paste is coated on the contact surface between the refractory high entropy alloy and the carbon material and the contact surface between the carbon material and the refractory pure metal.
[0016] The present invention also provides a sintering device for flash sintering of metal or metal-based composite materials, comprising a power supply, a sintering mold and the composite electrode of the present invention, wherein two composite electrodes are fixed in the sintering mold, and the power supply is respectively connected to the two composite electrodes.
[0017] According to the aspects described above and any possible implementation, an implementation is further provided, wherein the sintering mold is a cylindrical barrel-shaped body with a through hole, the two composite electrodes are respectively fixed on the upper and lower parts of the sintering mold, and the middle part of the sintering mold is used to place the metal or metal-based composite powder to be sintered.
[0018] According to the above aspects and any possible implementation, an implementation is further provided, wherein the power supply provides a pulse current, and the parameters of the pulse current are: frequency 1 Hz to 300000 Hz, pulse width 1 μs to 200 μs, current density 1 A / mm 2 ~1000A / mm 2 , power 10-500kw.
[0019] According to the above aspects and any possible implementation, an implementation is further provided, wherein the sintering mold is made of aluminum oxide, titanium carbide, boron nitride, titanium nitride ceramic or other ceramics.
[0020] The present invention also provides a flash sintering method for metal or metal-based composite materials, which is implemented by using the sintering device of the present invention, and comprises the following steps:
[0021] S1. The metal or metal-based composite powder to be sintered is filled into the middle of the sintering mold of the sintering device;
[0022] S2 inserts two composite electrode punches into the sintering mold from the upper and lower ends respectively, and applies a certain pressure to the two composite electrodes;
[0023] S3. Connect the two composite electrodes to the power supply of the sintering device respectively, and turn on the power supply to perform flash sintering.
[0024] According to the aspects described above and any possible implementation method, an implementation method is further provided, in which the pulse current parameters used in the sintering process are: frequency 300000 Hz, current 1500A, 1800A, 2500A or 2700A, pulse width 5μs, output power 20kW, 35kW, 40kW or 50kW.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] Compared with other existing current-assisted sintering methods, the present invention can utilize the huge amount of Joule heat generated by the self-heating carbon material in the composite electrode under the action of electric current, and make the temperature of the sintered powder rise sharply through conduction, thereby achieving complete densification of the metal or metal-based composite material in a very short time, greatly improving the preparation efficiency of the metal or metal-based composite material; during sintering, the present invention utilizes the composite electrode to generate a large amount of heat during the sintering process to provide it to the powder blank, thereby solving the problem that the metal powder flash burning process cannot generate enough Joule heat, and can achieve flash burning densification of the metal powder blank. This method can not only reduce the power requirement of the pulse power supply device for the flash sintering of metal powder, but also can flash burn to obtain larger metal or metal-based composite materials, solving the problem that large pieces of metal and metal-based composite materials cannot achieve flash burning densification. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the composite electrode structure of the present invention;
[0029] Figure 2 It is a schematic structural diagram of the sintering device of the present invention;
[0030] Figure 3 It is a schematic diagram of the method flow of the present invention. DETAILED DESCRIPTION
[0031] In order to better understand the technical solution of the present invention, the content of the present invention includes but is not limited to the specific implementation methods described below, and similar technologies and methods should be considered to be within the scope of protection of the present invention. In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments.
[0032] It should be clear that the embodiments described in the present invention are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The present invention provides a method for preparing a composite electrode, comprising the following steps:
[0034] (1) Cutting the refractory high entropy alloy, carbon material and refractory pure metal into required shapes, and cutting the selected refractory high entropy alloy, carbon material and refractory pure metal into required round bars or discs (the shape may also be square, triangle or other specific required shapes);
[0035] (2) Apply conductive silver paste to the contact interface between refractory high entropy alloy and carbon material and the contact interface between carbon material and refractory pure metal to ensure good electrical contact between different materials;
[0036] (3) The refractory high entropy alloy and the refractory pure metal are arranged at both ends, and the carbon material is arranged in the middle. After the three materials are stacked together, they are placed in a drying oven and baked at a certain temperature for a period of time to obtain a composite electrode, specifically, baked at 200 degrees for 2 hours.
[0037] like Figure 1 As shown, the present invention also provides a composite electrode for sintering, wherein the refractory high entropy alloy is arranged at the upper end of the composite electrode, and the length accounts for 50-80% of the entire composite electrode; the carbon material is arranged in the middle of the composite electrode, and the length accounts for 15-30% of the entire composite electrode; the refractory pure metal is arranged at the lower end of the composite electrode, and its thickness accounts for 5-20% of the entire composite electrode, and the thickness of the refractory pure metal is sufficient as long as it can ensure that it does not deform under pressure. Among them, the refractory high entropy alloy mainly maintains sufficient strength at high temperature, thereby providing sufficient pressure for the powder in the flash burning process; the self-heating carbon material generates a large amount of heat under the action of electric current to ensure that the temperature of the powder flash burning process rises sharply, thereby realizing the powder flash burning densification; the refractory pure metal can not only ensure the transfer of heat, but also prevent the carbon element from contaminating the sintered powder, and in addition, it can prevent the bonding or overflow of the liquid phase in the flash burning process during the flash burning process. The shape and size of the composite electrode are determined by the specific sintering part size and shape requirements. The composite electrode is mainly composed of a refractory high entropy alloy, whose thickness accounts for 50-80% of the entire electrode; the carbon material as a heating element accounts for 15-30% of the entire electrode; the thickness of the refractory pure metal is sufficient as long as it can ensure that it does not deform under pressure, and its thickness accounts for 5-20% of the entire electrode. Refractory high entropy alloy electrodes can use refractory high entropy alloys such as NbMoTaW, AlNbTiV, TaNbTiV as the parent material. Carbon materials can be selected from graphite paper, graphite blocks, graphite felt and other materials according to the calorific value requirements. Refractory pure metals can be selected from pure tungsten, pure tantalum, pure rhenium and other materials.
[0038] The power source is connected to the two electrodes through the wire, and the power source provides a pulse current, which flows through the electrodes to circulate the powder.
[0039] The present invention also provides a sintering device for flash sintering of metal or metal-based composite materials, comprising a power supply, a sintering mold and two composite electrodes, wherein the two composite electrodes are fixed in the sintering mold, and the power supply is respectively connected to the two composite electrodes.
[0040] The power source is a pulse generator power source, a copper wire wrapped with ceramic heat-insulating fibers is a wire, and two self-heating composite electrodes are round rods or other shapes and sizes; the ceramic mold material can be: aluminum oxide, titanium carbide, boron nitride, titanium nitride ceramics or other ceramics, and the sintering mold is a cylindrical barrel with a through hole, and the shape of the through hole is circular, rectangular or square. When the shape of the barrel through hole is circular, the inner diameter of the barrel is 12mm and the outer diameter is 50mm. The two composite electrodes are respectively fixed on the upper and lower parts of the sintering mold, and the middle part of the sintering mold is used to place the metal or metal-based composite powder to be sintered. The power supply provides a pulse current, and the parameters of the pulse current are: frequency 1Hz~300000Hz, pulse width 1μs~200μs, current density 1A / mm 2 ~1000A / mm 2 , power 10-500kw.
[0041] The present invention also provides a flash sintering method for metal or metal-based composite materials, which is implemented by a sintering device and comprises the following steps:
[0042] S1. The metal or metal-based composite powder to be sintered is filled into the middle of the sintering mold of the sintering device;
[0043] S2 inserts two composite electrode punches into the sintering mold from the upper and lower ends respectively, and applies a certain pressure to the two composite electrodes;
[0044] S3. Connect the two composite electrodes to the power supply of the sintering device respectively, and turn on the power supply to perform flash sintering.
[0045] Among them, the pulse current parameters used in the sintering process are: frequency 300000 Hz, current 1500A, 1800A, 2500A or 2700A, pulse width 5μs, output power 20kW, 35kW, 40kW or 50kW.
[0046] Specifically, the flash sintering method of metal and metal-based composite materials based on composite electrodes of the present invention comprises the following steps:
[0047] A conventional pulse generator is used as a power source, a composite self-heating electrode is prepared from refractory high entropy alloy, self-heating carbon material and refractory pure metal as a sintering electrode, and a cylinder with a central through hole made of alumina or other ceramic materials is used as a sintering mold.
[0048] First, fill the metal or metal-based composite powder to be sintered into the mold, and then use two composite self-heating electrode punches to insert the mold from the upper and lower ends respectively, and then provide pressure for the upper and lower electrodes. The pressure here is 10-1000MPa. Keep the sintering pressure unchanged during the sintering process, and then connect the two sets of electrodes to the positive and negative poles of the pulse power supply respectively, turn on the pulse power supply to start flash sintering.
[0049] Select appropriate pulse current parameters according to the specific metal or metal-based composite powder composition. The specific pulse current parameters that can be used are: frequency 1Hz~300000Hz, pulse width 1μs~200μs, current density 1A / mm 2 ~1000A / mm 2 , power 10-500kw, sintering time 5-600s. The pulse waveform used in the pulse treatment can be a variety of waveforms such as sharp wave, square wave, sine wave, etc.
[0050] Compared with other existing current-assisted sintering methods, the present invention can utilize the huge amount of Joule heat generated by the self-heating carbon material of the composite electrode under the action of the current, and make the temperature of the sintered powder rise sharply through conduction, thereby achieving complete densification of the metal or metal-based composite material in a very short time, greatly improving the preparation efficiency of the metal or metal-based composite material. At the same time, compared with the traditional metal flash burning technology, the present invention can greatly reduce the output power requirements of the pulse power supply; in addition, compared with the traditional metal flash burning technology, this technology can flash burn to obtain a larger metal or metal-based composite material.
[0051] Embodiment 1:
[0052] In this embodiment, W-Cu20 (W: 80wt%; Cu: 20wt%) mixed powder is flash sintered. The specific steps are as follows:
[0053] Step 1: Add 100 grams of W-Cu20 mixed powder into a mold made of titanium carbide with an inner diameter of 12 mm and an outer diameter of 50 mm, then insert two electrodes made of pure refractory high-entropy alloy with a diameter of 12 mm into the upper and lower ends of the mold, and then provide a pressure of 200 MPa to the two electrodes.
[0054] Step 2: Connect the pulse power supply to the two electrodes, set the pulse current parameters as follows: frequency 300000 Hz, current 1500 A, pulse width 5 μs, output power 20 kW, then turn on the pulse power supply to flash sinter the powder for 20 s.
[0055] Step 3: Mix the powders to achieve densification during sintering. After the mold is cooled naturally, take out the sintered block, and measure the density of the sample by Archimedes drainage method to be 88.7%.
[0056] Embodiment 2:
[0057] In this embodiment, W-Cu20 (W: 80wt%; Cu: 20wt%) mixed powder is flash sintered. The specific steps are as follows:
[0058] Step 1: Add 100 grams of W-Cu20 mixed powder into a mold made of titanium carbide with an inner diameter of 12 mm and an outer diameter of 50 mm, then insert two electrodes made of pure refractory high-entropy alloy with a diameter of 12 mm into the upper and lower ends of the mold, and then provide a pressure of 200 MPa to the two electrodes.
[0059] Step 2: Connect the pulse power supply to the two electrodes, set the pulse current parameters as follows: frequency 300000 Hz, current 2500 A, pulse width 5 μs, output power 40 kW, then turn on the pulse power supply to flash sinter the powder for 20 s.
[0060] Step 3: Mix the powders to achieve densification during sintering. After the mold is cooled naturally, take out the sintered block, and measure the density of the sample by Archimedes drainage method to be 95.2%.
[0061] Comparison between Example 2 and Example 1 shows that increasing the sintering current (ie, output power) can significantly improve the density of the sintered block, but cannot achieve complete density.
[0062] Embodiment 3:
[0063] In this embodiment, W-Cu20 (W: 80wt%; Cu: 20wt%) mixed powder is flash sintered. The specific steps are as follows:
[0064] Step 1: Add 100 grams of W-Cu20 mixed powder into a mold made of titanium carbide with an inner diameter of 12 mm and an outer diameter of 50 mm, then insert two self-heating composite electrodes with a diameter of 12 mm into the upper and lower ends of the mold, and then provide a pressure of 200 MPa to the two electrodes.
[0065] Step 2: Connect the pulse power supply to the two electrodes, set the pulse current parameters as follows: frequency 300000 Hz, current 2500 A, pulse width 5 μs, output power 40 kW, then turn on the pulse power supply to flash sinter the powder for 20 s.
[0066] Step 3: Mix the powders to achieve densification during sintering. After the mold is cooled naturally, take out the sintered block, and measure the density of the sample by Archimedes drainage method to be 99.8%.
[0067] Comparison between Example 3 and Example 2 shows that under the same sintering pulse parameters, the use of a self-heating composite electrode can greatly improve the density of the sintered block and obtain a completely dense sintered block.
[0068] Embodiment 4:
[0069] In this embodiment, W-Cu20 (W: 80wt%; Cu: 20wt%) mixed powder is flash sintered. The specific steps are as follows:
[0070] Step 1: Add 200g of W-Cu20 mixed powder into the inner hole of 30×30mm 2 A square, 50mm outer diameter titanium carbide mold is then used with two 30×30mm 2 The square self-heating composite electrodes are inserted into the upper and lower ends of the mold, and then a pressure of 200MPa is applied to the two electrodes.
[0071] Step 2: Connect the pulse power supply to the two electrodes, set the pulse current parameters as follows: frequency 300000 Hz, current 2700 A, pulse width 5 μs, output power 50 kW, then turn on the pulse power supply to flash sinter the powder, and the sintering time is 20 s.
[0072] Step 3: Mix the powders to achieve densification during sintering. After the mold is cooled naturally, take out the sintered block, and measure the density of the sample by Archimedes drainage method to be 99.5%.
[0073] Comparison between Example 4 and Example 3 shows that without significantly increasing the output power of the pulse current device, a completely dense bulk W-Cu20 composite material can be sintered using a self-heating composite electrode.
[0074] Embodiment 5:
[0075] In this embodiment, WC-Co12 (WC: 80wt%; Co: 12wt%) mixed powder is flash sintered. The specific steps are as follows:
[0076] Step 1: Add 200g of WC-Co12 mixed powder into the inner hole of 30×30mm 2 A square, 50mm outer diameter titanium carbide mold is then used with two 30×30mm 2 The square self-heating composite electrodes are inserted into the upper and lower ends of the mold, and then a pressure of 200MPa is applied to the two electrodes.
[0077] Step 2: Connect the pulse power supply to the two electrodes, set the pulse current parameters as follows: frequency 300000 Hz, current 1800 A, pulse width 5 μs, output power 35 kW, then turn on the pulse power supply to flash sinter the powder, and the sintering time is 20 s.
[0078] Step 3: Mix the powders to achieve densification during sintering. After the mold is cooled naturally, take out the sintered block, and measure the density of the sample by Archimedes drainage method to be 99.7%.
[0079] Example 5 illustrates that the method and device for flash sintering of metals and metal-based composite materials based on composite electrode heating of the present invention can realize rapid preparation of different metal-based composite powder materials.
[0080] The above description is only a specific implementation method of the present invention for W-Cu20 composite materials and WC-Co12 composite materials, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, can replace similar materials, equipment or adjust relevant technical parameters according to the technical solution and inventive concept of the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A composite electrode for sintering, It is characterized in that The composite electrode comprises: a refractory high entropy alloy, a carbon material and a refractory pure metal, wherein: The refractory high entropy alloy is arranged at the upper end of the composite electrode, and its length accounts for 50-80% of the entire composite electrode. The material of the refractory high entropy alloy is one of NbMoTaW, AlNbTiV, and TaNbTiV; The carbon material is arranged in the middle of the composite electrode, and its length accounts for 15-30% of the entire composite electrode; The refractory pure metal is arranged at the lower end of the composite electrode, and its length accounts for 5-20% of the entire composite electrode. The refractory pure metal is made of one of pure tungsten, pure tantalum and pure rhenium, and is prepared by the following method: (1) cutting the refractory high entropy alloy, carbon material and refractory pure metal into required shapes; (2) Applying conductive silver paste on the contact interface between refractory high entropy alloy and carbon material and the contact interface between carbon material and refractory pure metal; (3) The refractory high entropy alloy and the refractory pure metal are placed at both ends, and the carbon material is placed in the middle. After the three materials are stacked together, they are placed in a drying oven and baked at a certain temperature for a period of time to obtain a composite electrode.
2. The composite electrode according to claim 1, It is characterized in that The carbon material is made of one of graphite paper, graphite block and graphite felt.
3. A sintering device for flash sintering of metal or metal matrix composite materials, It is characterized in that It comprises a power supply, a sintering mold and the composite electrode according to any one of claims 1 to 2, wherein two composite electrodes are fixed in the sintering mold, and the power supply is connected to the two composite electrodes respectively.
4. The sintering device according to claim 3, It is characterized in that The sintering mold is a cylindrical barrel-shaped body with a through hole. The two composite electrodes are respectively fixed on the upper and lower parts of the sintering mold. The middle part of the sintering mold is used to place the metal or metal-based composite powder to be sintered.
5. The sintering device according to claim 3, It is characterized in that The power supply provides a pulse current, and the parameters of the pulse current are: frequency 1Hz~300000Hz, pulse width 1μs~200μs, current density 1A / mm 2 ~1000A / mm 2 , power 10-500kw.
6. The sintering device according to claim 3, It is characterized in that The sintering mold is made of alumina, titanium carbide, boron nitride or titanium nitride ceramic.
7. A method for flash sintering of metal or metal matrix composite materials, It is characterized in that The method is implemented by using the sintering device according to any one of claims 3 to 6, and the method comprises the following steps: S1. The metal or metal-based composite powder to be sintered is filled into the middle of the sintering mold of the sintering device; S2 inserts two composite electrode punches into the sintering mold from the upper and lower ends respectively, and applies a certain pressure to the two composite electrodes; S3. Connect the two composite electrodes to the power supply of the sintering device respectively, and turn on the power supply to perform flash sintering.
8. The method according to claim 7, It is characterized in that The pulse current parameters used in the sintering process are: frequency 300000 Hz, current 1500A, 1800A, 2500A or 2700A, pulse width 5μs, output power 20kW, 35kW, 40kW or 50kW.