A method for preparing antibacterial and antiviral yarn with a core-shell structure

The method for preparing antibacterial and antiviral yarn with a core-shell structure solves the problems of easy shedding and short service life of existing antibacterial and antiviral materials, achieving long-term antibacterial effect and biosafety, and is suitable for a variety of textiles and medical and health protective products.

CN115748052BActive Publication Date: 2026-11-17CONSINEE GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211507190.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2026-11-17
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Existing antibacterial and antiviral materials are prone to detachment from fibers and clothing products, have a short service life, cannot meet commercialization requirements, and have problems such as poor heat resistance, easy development of drug resistance and toxicity.

Method used

An antibacterial and antiviral yarn preparation method with a core-shell structure is adopted. By configuring an antibacterial and antiviral shell precursor, mixing nano-inorganic metal oxides, inorganic oxide modified materials and natural Chinese medicine preparations, a shell fiber treatment liquid is formed. Subsequently, it is treated with textile fibers to form antibacterial functional fibers. Combined with water-soluble fibers and core-fixed yarn structure, the long-term effectiveness of antibacterial materials is ensured.

Benefits of technology

It achieves antibacterial and antiviral yarn that retains its high antibacterial ability after multiple washes, has broad-spectrum antibacterial properties, good biosafety, and yarn strength that meets textile usage requirements, making it suitable for a variety of clothing and medical protective products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for preparing antibacterial and antiviral yarn with a core-shell structure, relating to the field of textile technology. The method includes multiple steps such as preparing an antibacterial and antiviral shell precursor, preparing antibacterial and antiviral yarn, and preparing an antibacterial composite yarn. Compared with existing technologies, the antibacterial and antiviral fibers and yarns of this application can be widely used in processing various antibacterial and antiviral civilian protective clothing and other products to meet the needs of home, outdoor, and professional textile and apparel products. They can also be used in various medical and health protective products. Furthermore, the special yarn structure allows this yarn to have a service life far exceeding that of existing similar antibacterial yarns, in addition to meeting general antibacterial and antiviral requirements, truly achieving water resistance and possessing significant social and economic importance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile technology, and more particularly to the field of antibacterial functional textile technology. Background Technology

[0002] In recent years, people have placed greater emphasis on antibacterial and antiviral fibers and clothing products. Currently, antibacterial and antiviral materials mainly include those that are highly effective, non-toxic, and broad-spectrum. There are three main categories of antibacterial and antiviral materials used in fibers and clothing: First, organic antibacterial agents. These are mostly complex compounds containing elements such as nitrogen, sulfur, and chlorine, including quaternary ammonium salts, biguanides, alcohols, phenols, aldehydes, organometallic compounds, arsenic, and thiophenes. These antibacterial agents have a fast bactericidal speed, good short-term bactericidal effect, and are easy to process. However, they have poor heat stability, are prone to developing drug resistance, and their decomposition products are toxic. Second, inorganic antibacterial agents mainly refer to metals such as silver, copper, and zinc, or their ions, attached to fibers and fabrics. These antibacterial agents have good heat resistance, broad-spectrum antibacterial activity, long effective antibacterial period, low toxicity, and do not develop drug resistance. However, silver-based antibacterial agents are prone to discoloration and have poor antifungal and antimold effects. The toxicity and safety of heavy metal ions are controversial and have been banned in Western countries. Thirdly, there are natural antibacterial agents. These are mainly extracted from animals, such as chitin, chitosan, and insect antibacterial proteins, and from plants, such as juniper, artemisia, and aloe. These antibacterial agents are highly effective against some bacteria and are safe and non-toxic, but their antibacterial activity is limited, lacks broad-spectrum activity, is difficult to process, has poor heat resistance, and a short lifespan.

[0003] Another major problem with the aforementioned antibacterial and antiviral materials is that the antibacterial and antiviral materials will fall off from the fibers after prolonged use or washing, resulting in a short overall service life and failing to meet the requirements for true commercial use. Summary of the Invention

[0004] This invention addresses the shortcomings of existing technologies by providing a method for preparing antibacterial and antiviral yarn with a core-shell structure. The antibacterial and antiviral fibers and yarns of this application can be widely used in processing various antibacterial and antiviral civilian protective clothing and other products to meet the needs of home, outdoor, and professional textile and apparel products. They can also be used in various medical and health protective products. Furthermore, the unique yarn structure allows this yarn to not only meet general antibacterial and antiviral requirements but also have a service life far exceeding that of existing similar antibacterial yarns, truly achieving water resistance and possessing significant social and economic value.

[0005] To solve the above-mentioned technical problems, the present invention provides a method for preparing antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, by weight, 0.05-1.2 parts of nano-inorganic metal oxide powder, 0.5-6.0 parts of nano-inorganic oxide modified material, 0.5-3.0 parts of natural Chinese medicine preparation, 29.8-38.95 parts of chitin protein, and 50-70 parts of deionized water are placed in a reaction vessel and stirred at 800-3000 rpm at a temperature of 80-90°C for 1.5-3 hours; Step B: By weight, 40-60 parts of antibacterial... A shell precursor is mixed with 40-60 parts softened water to form a shell fiber treatment solution, which is then used to treat textile fibers to form antibacterial functional fibers; Step C: The antibacterial functional fibers are made into antibacterial functional yarns; Step D: 70%-90% of textile fibers and 10%-15% of water-soluble fibers are mixed by weight to form blended fibers, which are then made into water-soluble blended yarns; Step E: The antibacterial functional yarn is selected as the core yarn using a fancy twisting machine, and several water-soluble blended yarns are used as fixing yarns to form an antibacterial composite yarn; Step F: The antibacterial composite yarn is washed with water to dissolve the water-soluble fibers within it; Step G: The antibacterial composite yarn is dried.

[0006] In the above technical solution, preferably, in step A, the nano-inorganic metal oxide powder is aluminum oxide, silicon dioxide, or a mixture thereof with a particle size of 15.3 nm to 91.6 nm; the nano-inorganic oxide modifying material is an organosilicon surfactant, which includes cationic, anionic, nonionic, and amphoteric dimethylsiloxane series surfactants; the natural Chinese medicine preparation is a mixture of powders of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria with a particle size greater than 200 mesh.

[0007] In the above technical solution, preferably, in step B, in the dyeing machine, the mass ratio of the shell fiber treatment solution to the textile fiber is between 1:1 and 10. Then, the machine is turned on to conduct a water bath on the textile fiber. The water bath temperature is between 80°C and 90°C, and the reaction time is between 1.5 hours and 3 hours. After the water bath, the textile fiber is dehydrated and then dried using a hot air or drum dryer. During the drying process, the temperature of the last section is controlled at 120°C to 130°C.

[0008] In the above technical solution, preferably, in step B, the mass ratio of shell fiber treatment liquid to textile fiber in the sizing machine is between 1:1 and 10. Then, the machine is started to continuously perform liquid-pinching treatment on the textile fiber, and the liquid-pinching rate is controlled at 70% to 90%. Then, a hot air or drum dryer is used for drying. During drying, the temperature of the last section is controlled at 120℃ to 130℃, and the rest is carried out according to the conventional sizing process.

[0009] In the above technical solution, preferably, in step D, the water-soluble fiber is polyvinyl alcohol fiber.

[0010] In the above technical solution, preferably, in step B, the textile fiber includes fibers formed by single or blended fabrics of cotton, wool, silk, linen, polyester, nylon, acrylic, and viscose.

[0011] In the above technical solution, preferably, when the textile fiber is cashmere or wool fiber, in step C, the antibacterial functional fiber is blended, first opened by an opening machine, then sulphurized with wool oil for at least 10 hours, and the moisture regain on the machine is controlled within 15% ± 5% during blending; the blended fiber is combed, with a combing zone spacing of 7-10 filaments; the blended fiber is finely spun, with a back zone draft ratio of 1.15-1.35, a fine spinning machine speed of 6000 rpm-8500 rpm, and a back zone spacing of 60 mm-75 mm; the blended fiber is wound, with a spinning speed between 250 m / min and 650 m / min; the blended fiber is doubling, with a spinning speed between 250 m / min and 650 m / min, and a fixed length of 14300 m; the blended fiber is twisted, with a spinning speed between 5000 rpm and 7000 rpm, and a twist direction of " Z".

[0012] In the above technical solution, preferably, the wool-refining agent includes 3% FX-906 and wool oil, and 1.5% FX-AS301 antistatic agent.

[0013] In the above technical solution, preferably, in step D, 85% to 90% of cashmere or wool fibers and 10% to 15% of water-soluble fibers are selected by mass percentage to form a blended fiber, which is then processed through the steps of blending, combing, spinning, and twisting to form a water-soluble blended yarn.

[0014] In the above technical solution, preferably, after the antibacterial composite yarn is washed with water in step F, it is then treated with a shell fiber treatment solution to further treat the antibacterial composite yarn.

[0015] This application utilizes a unique core-fixed yarn structure to conceal antibacterial and antiviral materials within the yarn. Because the core yarn is encased in the fixed yarn, even if the antibacterial and antiviral materials detach during wear and washing, they remain within the fixed yarn, maximizing their retention on clothing. This retention rate is significantly higher than that of antibacterial and antiviral materials coated on the yarn surface. Simultaneously, the fixed yarn contains water-soluble fibers. When these fibers dissolve, gaps appear in the fixed yarn, exposing or transferring the antibacterial and antiviral materials from the core yarn to the fixed yarn surface, thus providing overall antiviral and antibacterial protection. Furthermore, the water-soluble fibers constitute only 10% to 15% of the fixed yarn fibers. The core-fixed yarn structure itself strengthens the yarn, ensuring that even if all the water-soluble fibers dissolve, the overall strength of the core-fixed yarn meets textile and usage requirements. If the fixed yarn is wool or cashmere, the yarn even exhibits a plush texture.

[0016] The antibacterial finishing agent in this application is a combination of natural Chinese herbal medicines and natural minerals. Fibers treated with this antibacterial finishing agent achieve a long-lasting antibacterial effect, maintaining good antibacterial ability even after multiple washes, while posing no physiological toxicity to humans. Fabrics made using this fiber and yarn exhibit highly efficient, broad-spectrum antibacterial and antiviral properties, as well as excellent biocompatibility. The antibacterial fiber in this application is simple to manufacture, has good physical properties, is suitable for various weaving methods, and has a wide range of applications.

[0017] Knitted fabrics prepared using the antibacterial yarns and fibers of this invention exhibit an inhibition rate of over 90% against Staphylococcus aureus, Escherichia coli, and Candida albicans after 50 washes, and all other basic physical and mechanical properties meet the requirements of the national first-class standard. The antibacterial fibers and yarns of this application can be widely used in the processing of various health-functional textiles to meet the needs of daily clothing, medical protective equipment, household, outdoor, and occupational textile products, and have significant social and economic implications.

[0018] Compared with existing technologies, the antibacterial and antiviral fibers and yarns of this application can be widely used in the processing of various antibacterial and antiviral civilian protective clothing and other products to meet the needs of textile and apparel products for home, outdoor, and professional use. They can also be used in various medical and health protective products. At the same time, the special yarn structure enables this yarn to have a service life far exceeding that of existing similar antibacterial yarns, in addition to meeting general antibacterial and antiviral requirements, truly achieving water resistance, which has significant social and economic implications. Detailed Implementation

[0019] Example 1: A method for preparing an antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, by weight, 1.2 parts of nano-inorganic metal oxide powder, 6.0 parts of nano-inorganic oxide modified material, 3.0 parts of natural Chinese herbal medicine preparation, 29.8 parts of chitin protein, and 60 parts of deionized water. In a reaction vessel, the mixture is stirred at 3000 rpm at 90°C for 3 hours. The nano-inorganic metal oxide powder is a mixture of 15.3 nm aluminum oxide and 25.6 nm silicon dioxide in a 1:1 weight ratio; the nano-inorganic oxide modified material is a cationic dimethylsiloxane surfactant. The natural Chinese herbal medicine preparation is a mixture of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria in a 25% weight ratio, processed into a 250-mesh ultrafine powder.

[0020] Step B: By weight, 40 parts of antibacterial and antiviral shell precursor are mixed with 60 parts of softened water to form a shell fiber treatment solution. This solution is then used to treat textile fibers to form antibacterial functional fibers, specifically wool fibers. In a dyeing machine, the mass ratio of the shell fiber treatment solution to the wool fibers is maintained at 1:8. The machine is then turned on to subject the wool fibers to a water bath at 80°C for 1.5 hours. After the water bath, the wool fibers are dehydrated and then dried using a hot air or drum dryer. The temperature of the final drying stage is controlled at 130°C.

[0021] Step C: Prepare antibacterial functional fibers into antibacterial functional yarn; perform blending of the antibacterial functional fibers, first opening them with an opening machine, then adding wool oil and allowing them to absorb the fibers for at least 10 hours, controlling the moisture regain on the machine to within 10% ± 5% during blending; comb the blended fibers, with a combing zone spacing of 7-10 filaments; perform fine spinning of the blended fibers, with a back zone draft ratio of 1.05-1.45, a fine spinning machine speed of 5500 rpm-8500 rpm, and a back zone spacing of 40 mm-80 mm; perform winding of the blended fibers, with a spinning speed between 250 m / min and 650 m / min; perform doubling of the blended fibers, with a spinning speed between 250 m / min and 650 m / min, and a fixed length of 14300 m; perform double twisting of the blended fibers, with a spinning speed between 5000 rpm and 8000 rpm and a twist direction of "Z". The wool-smoothing agent comprises 3% FX-906 and wool oil, and 1.5% FX-AS301 antistatic agent.

[0022] Step D: By weight percentage, select 85% cashmere and 15% water-soluble fiber to form a blended fiber, and then make the water-soluble fiber into a water-soluble blended yarn; the water-soluble fiber is polyvinyl alcohol fiber. For blended fibers, the process involves first mixing and layering cashmere twice, then adding a blending agent and beating once more. The water-soluble fibers are then opened separately. Next, the pre-bleached cashmere is layered and mixed with the opened water-soluble fibers twice, with bagging performed during the mixing process. After mixing, the fibers proceed directly to the carding process. The moisture regain during the carding process is controlled between 10% and 19%. For the carding of blended fibers, the speed ratio between the cylinder and the work roll is between 360 / 2.5 and 180 / 2.5, the speed ratio between the cylinder and the doffer is between 360 / 21 and 340 / 17, the distance between the cylinder and the work roll is between 1.3 mm and 1.6 mm, and the distance between the cylinder and the doffer is between 0.2 mm and 0.65 mm. For the spinning of blended fibers, the draft ratio is between 1.05 and 1. The yarn twist is between 0.45 and 300T / M to 500T / M, with a twist direction of "Z" and a spindle speed between 6500 rpm and 7000 rpm. For blended fibers, a winding and twisting process is performed, with the spinning speed during winding between 400m / min and 650m / min, and the spinning speed during doubling between 5500 rpm and 6500 rpm, with a twist between 200T / M and 400T / M and a twist direction of "S".

[0023] Step E: Using a fancy twisting machine, select an antibacterial functional yarn as the core yarn and several water-soluble blended yarns as the binding yarn to make an antibacterial composite yarn; wherein the hollow spindle twist is 400 T / M to 700 T / M, twist direction "Z", the external twist is 200 T / M to 400 T / M, twist direction "S", the overfeed ratio is 2, the draft ratio is 5 times to 20 times, and the core yarn tension is 0.5% to 5.5%.

[0024] Step F: Wash the antibacterial composite yarn with water to dissolve the water-soluble fibers within it; the washing temperature should be 40℃ or higher. After washing, treat the antibacterial composite yarn with a shell fiber treatment solution, either by spraying or impregnation. Spraying involves applying the shell fiber treatment solution to the surface of the antibacterial composite yarn, while impregnation involves bathing the antibacterial composite yarn in the shell fiber treatment solution. Step G: Dry the antibacterial composite yarn.

[0025] The antibacterial composite yarn from Example 1 was prepared into a 160-280 g / m² knitted fabric. According to Appendix D of FZ / T73023-2006, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were all greater than 96%. After 50 washes, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were all greater than 90%. According to ISO18184:2014, the N1H1 influenza virus activity value was greater than 3.0. After 50 washes, the N1H1 influenza virus activity value was greater than 2.0. According to GB18401-2003 standard requirements, it meets Class A requirements, i.e., requirements for infant and toddler products.

[0026] Example 2: A method for preparing an antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, comprising, by weight, 0.05 parts of nano-inorganic metal oxide powder, 0.5 parts of nano-inorganic oxide modified material, 0.5 parts of natural Chinese herbal medicine preparation, 38.95 parts of chitin protein, and 60 parts of deionized water. The mixture is stirred at 800 rpm and reacted at 80°C for 1.5 hours in a reaction vessel. The nano-inorganic metal oxide powder is a mixture of 91.6 nm aluminum oxide and 42.6 nm silicon dioxide in an 80 / 20 weight ratio; the nano-inorganic oxide modified material is a nonionic betaine dimethylsiloxane surfactant. The natural Chinese herbal medicine preparation is a mixture of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria in a different weight ratio of 20:20:20:40, processed into a 300-mesh ultrafine powder.

[0027] Step B: By weight, mix 60 parts of antibacterial and antiviral shell precursor with 40 parts of softened water to form a shell fiber treatment solution. Then, treat the textile fibers with this solution to form antibacterial functional fibers. The textile fibers are a blend of cashmere and cotton fibers in an 80 / 20 weight ratio. In a dyeing machine, maintain the shell fiber treatment solution to textile fiber weight ratio at 1:8. Then, start the machine and subject the blended wool to a water bath at 80°C for 1.5 hours. After the water bath, dehydrate the blended wool and then dry it using a hot air or drum dryer. The temperature of the final drying stage is controlled at 120°C. Step C: Produce antibacterial functional yarn from the blended wool.

[0028] Step D: By weight percentage, select 90% cashmere and 10% water-soluble fiber to form a blended fiber, and then make the water-soluble fiber into a water-soluble blended yarn; the water-soluble fiber is polyvinyl alcohol fiber. For blended fibers, the process involves first mixing and layering cashmere twice, then adding a blending agent and beating once more. The water-soluble fibers are then opened separately. Next, the pre-bleached cashmere is layered and mixed with the opened water-soluble fibers twice, with bagging performed during the mixing process. After mixing, the fibers proceed directly to the carding process. The moisture regain during the carding process is controlled between 10% and 19%. For the carding of blended fibers, the speed ratio between the cylinder and the work roll is between 360 / 2.5 and 180 / 2.5, the speed ratio between the cylinder and the doffer is between 360 / 21 and 340 / 17, the distance between the cylinder and the work roll is between 1.3 mm and 1.6 mm, and the distance between the cylinder and the doffer is between 0.2 mm and 0.65 mm. For the spinning of blended fibers, the draft ratio is between 1.05 and 1. The yarn twist is between 0.45 and 300 T / M to 500 T / M, with a twist direction of "Z" and a spindle speed between 6500 rpm and 7000 rpm. For blended fibers, a winding and twisting process is performed, with the winding speed between 400 m / min and 650 m / min during winding and the speed between 5500 rpm and 6500 rpm during doubling, with a twist between 200 T / M and 400 T / M and a twist direction of "S".

[0029] Step E: Using a fancy twisting machine, select an antibacterial functional yarn as the core yarn and several water-soluble blended yarns as the binding yarn to make an antibacterial composite yarn; wherein the hollow spindle twist is 400 T / M to 700 T / M, twist direction "Z", the external twist is 200 T / M to 400 T / M, twist direction "S", the overfeed ratio is 2, the draft ratio is 5 times to 20 times, and the core yarn tension is 0.5% to 5.5%.

[0030] Step F: Wash the antibacterial composite yarn with water to dissolve the water-soluble fibers within it; the washing temperature should be 40℃ or higher. After washing, treat the antibacterial composite yarn with a shell fiber treatment solution, either by spraying or impregnation. Spraying involves applying the shell fiber treatment solution to the surface of the antibacterial composite yarn, while impregnation involves bathing the antibacterial composite yarn in the shell fiber treatment solution. Step G: Dry the antibacterial composite yarn.

[0031] The antibacterial composite yarn from Example 2 was used to prepare a 160 g / m² knitted fabric. According to Appendix D of FZ / T73023-2006, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were greater than 99%, greater than 99%, and 98%, respectively. After 50 washes, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were greater than 99%, greater than 99%, and 96%, respectively. According to ISO 18184:2014, the N1H1 influenza virus activity value was 3.0; after 50 washes, the N1H1 influenza virus activity value was 2.3. According to GB 18401-2003 standard requirements, it meets Class A requirements.

[0032] Example 3: A method for preparing an antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, by weight, 0.6 parts of nano-inorganic metal oxide powder, 3.0 parts of nano-inorganic oxide modified material, 1.5 parts of natural Chinese herbal medicine preparation, 35.9 parts of chitin protein, and 60 parts of deionized water. In a reaction vessel, the mixture is stirred at 2000 rpm and reacted at 85°C for 2.5 hours. The nano-inorganic metal oxide powder is aluminum oxide with a particle size of 42.8 nanometers; the nano-inorganic oxide modified material is anionic dimethylsiloxane activator. The natural Chinese herbal medicine preparation is a mixture of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria in a weight ratio of 30:20:30:20, processed into an ultrafine powder larger than 220 mesh.

[0033] Step B: By weight, 50 parts of antibacterial and antiviral shell precursor are mixed with 50 parts of softened water to form a shell fiber treatment solution. This solution is then used to treat textile fibers to form antibacterial functional fibers. The textile fibers are pre-treated 60-count cotton-linen-polyester (50 / 30 / 20) yarn. The yarn is continuously processed in a sizing machine, with the liquid extraction rate controlled at 80%. The temperature is adjusted to 125℃ in the final drying stage, while the rest of the process follows conventional sizing procedures. The final product is the antibacterial functional yarn.

[0034] Step C: By weight percentage, select 85% cashmere and 15% water-soluble fiber to form a blended fiber, and then make the water-soluble fiber into a water-soluble blended yarn; the water-soluble fiber is polyvinyl alcohol fiber. For blended fibers, the process involves first mixing and layering cashmere twice, then adding a blending agent and beating once more. The water-soluble fibers are then opened separately. Next, the pre-bleached cashmere is layered and mixed with the opened water-soluble fibers twice, with bagging performed during the mixing process. After mixing, the fibers proceed directly to the carding process. The moisture regain during the carding process is controlled between 10% and 19%. For the carding of blended fibers, the speed ratio between the cylinder and the work roll is between 360 / 2.5 and 180 / 2.5, the speed ratio between the cylinder and the doffer is between 360 / 21 and 340 / 17, the distance between the cylinder and the work roll is between 1.3 mm and 1.6 mm, and the distance between the cylinder and the doffer is between 0.2 mm and 0.65 mm. For the spinning of blended fibers, the draft ratio is between 1.05 and 1. The yarn twist is between 0.45 and 300T / M to 500T / M, with a twist direction of "Z" and a spindle speed between 6500 rpm and 7000 rpm. For blended fibers, a winding and twisting process is performed, with the spinning speed during winding between 400m / min and 650m / min, and the spinning speed during doubling between 5500 rpm and 6500 rpm, with a twist between 200T / M and 400T / M and a twist direction of "S".

[0035] Step E: Using a fancy twisting machine, select an antibacterial functional yarn as the core yarn and several water-soluble blended yarns as the binding yarn to make an antibacterial composite yarn; wherein the hollow spindle twist is 400 T / M to 700 T / M, twist direction "Z", the external twist is 200 T / M to 400 T / M, twist direction "S", the overfeed ratio is 2, the draft ratio is 5 times to 20 times, and the core yarn tension is 0.5% to 5.5%.

[0036] Step F: Wash the antibacterial composite yarn with water to dissolve the water-soluble fibers within it; the washing temperature should be 40℃ or higher. After washing, treat the antibacterial composite yarn with a shell fiber treatment solution, either by spraying or impregnation. Spraying involves applying the shell fiber treatment solution to the surface of the antibacterial composite yarn, while impregnation involves bathing the antibacterial composite yarn in the shell fiber treatment solution. Step G: Dry the antibacterial composite yarn.

[0037] The antibacterial composite yarn from Example 3 was used to prepare a 180 g / m² knitted fabric. According to Appendix D of FZ / T73023-2006, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were all greater than 99%. After 50 washes, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were all greater than 99%. According to ISO18184:2014, the N1H1 influenza virus activity value was 3.2. After 50 washes, the N1H1 influenza virus activity value was 2.8. According to GB18401-2003 standard requirements, it meets Class A requirements.

[0038] Example 4: A method for preparing an antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, by weight ratio, 0.8 parts of nano-inorganic metal oxide powder, 4.0 parts of nano-inorganic oxide modified material, 2.0 parts of natural Chinese medicine preparation, 33.2 parts of chitin protein, and 60 parts of deionized water. In a reaction vessel, the mixture is stirred at 1000 rpm and reacted at 85°C for 2 hours. The nano-inorganic metal oxide powder is a mixture of 25.3 nm aluminum oxide and 38.9 nm silicon dioxide in a weight ratio of 40:60. The nano-inorganic oxide modified material is a mixture of 50% cationic and 50% nonionic dimethylsiloxane series active agents. The natural Chinese medicine preparation is a mixture of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria in a weight ratio of 23:27:27:23, processed into an ultrafine powder larger than 250 mesh.

[0039] Step B: By weight, 43 parts of antibacterial and antiviral shell precursor are mixed with 57 parts of softened water to form a shell fiber treatment solution. This solution is then used to treat textile fibers to form antibacterial functional fibers. The textile fibers are 32-count cashmere / silk / acrylic yarn. In a yarn dyeing machine, the mass ratio of the shell fiber treatment solution to the wool fiber is maintained at 1:10. The wool fibers are then subjected to a water bath at 83°C for 2 hours. After the water bath, the wool fibers are dehydrated and then dried using a hot air or drum dryer. The temperature of the final drying stage is controlled at 120°C.

[0040] Step C: By weight percentage, select 85% cashmere and 15% water-soluble fiber to form a blended fiber, and then make the water-soluble fiber into a water-soluble blended yarn; the water-soluble fiber is polyvinyl alcohol fiber. For blended fibers, the process involves first mixing and layering cashmere twice, then adding a blending agent and beating once more. The water-soluble fibers are then opened separately. Next, the pre-bleached cashmere is layered and mixed with the opened water-soluble fibers twice, with bagging performed during the mixing process. After mixing, the fibers proceed directly to the carding process. The moisture regain during the carding process is controlled between 10% and 19%. For the carding of blended fibers, the speed ratio between the cylinder and the work roll is between 360 / 2.5 and 180 / 2.5, the speed ratio between the cylinder and the doffer is between 360 / 21 and 340 / 17, the distance between the cylinder and the work roll is between 1.3 mm and 1.6 mm, and the distance between the cylinder and the doffer is between 0.2 mm and 0.65 mm. For the spinning of blended fibers, the draft ratio is between 1.05 and 1. The yarn twist is between 0.45 and 300 T / M to 500 T / M, with a twist direction of "Z" and a spindle speed between 6500 rpm and 7000 rpm. For blended fibers, a winding and twisting process is performed, with the winding speed between 400 m / min and 650 m / min during winding and the speed between 5500 rpm and 6500 rpm during doubling, with a twist between 200 T / M and 400 T / M and a twist direction of "S".

[0041] Step D: Using a fancy twisting machine, select an antibacterial functional yarn as the core yarn and several water-soluble blended yarns as the fixing yarn to make an antibacterial composite yarn; wherein the hollow spindle twist is 400 T / M~700 T / M, twist direction "Z", the external twist is 200 T / M~400 T / M, twist direction "S", the overfeed ratio is 2, the draft ratio is 5 times to 20 times, and the core yarn tension is 0.5%~5.5%.

[0042] Step E: Wash the antibacterial composite yarn with water to dissolve the water-soluble fibers within it; the washing temperature should be 40℃ or higher. After washing, treat the antibacterial composite yarn with a shell fiber treatment solution, either by spraying or impregnation. Spraying involves applying the shell fiber treatment solution to the surface of the antibacterial composite yarn, while impregnation involves bathing the antibacterial composite yarn in the shell fiber treatment solution. Step G: Dry the antibacterial composite yarn.

[0043] The antibacterial composite yarn from Example 4 was used to prepare a 200 g / m² knitted fabric. According to Appendix D of FZ / T73023-2006, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were all greater than 99%. After 50 washes, the inhibition rates against Staphylococcus aureus, Escherichia coli, and Candida albicans were greater than 99%, 98%, and 97%, respectively. According to ISO18184:2014, the N1H1 influenza virus activity value was 3.3. After 50 washes, the N1H1 influenza virus activity value was 2.8. According to the requirements of GB18401-2003 standard, it meets the Class A requirements.

[0044] Example 5: A method for preparing an antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, by weight ratio, 0.05 parts of nano-inorganic metal oxide powder, 0.5 parts of nano-inorganic oxide modified material, 0.5 parts of natural Chinese medicine preparation, 29.8 parts of chitin protein, and 50 parts of deionized water. In a reaction vessel, the mixture is stirred at 800 rpm and reacted at 80°C for 1.5 hours. The nano-inorganic metal oxide powder is a mixture of 25.3 nm aluminum oxide and 38.9 nm silicon dioxide in a weight ratio of 40:60. The nano-inorganic oxide modified material is a mixture of 50% cationic and 50% nonionic dimethylsiloxane series active agents. The natural Chinese medicine preparation is a mixture of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria in a weight ratio of 23:27:27:23, processed into an ultrafine powder larger than 250 mesh. Step B: By weight, 40 parts of antibacterial and antiviral shell precursor are mixed with 60 parts of softened water to form a shell fiber treatment solution. This solution is then used to treat textile fibers to form antibacterial functional fibers. The textile fibers are polyester yarn. In a yarn dyeing machine, the mass ratio of the shell fiber treatment solution to wool fibers is maintained at 1:10. The wool fibers are then subjected to a water bath at 83°C for 2 hours. After the water bath, the wool fibers are dehydrated and then dried using a hot air or drum dryer. The temperature of the final drying stage is controlled at 120°C.

[0045] Step C: By weight percentage, select 90% cashmere and 10% water-soluble fiber to form a blended fiber, and then make the water-soluble fiber into a water-soluble blended yarn; the water-soluble fiber is polyvinyl alcohol fiber. For blended fibers, the process involves first mixing and layering cashmere twice, then adding a blending agent and beating once more. The water-soluble fibers are then opened separately. Next, the pre-bleached cashmere is layered and mixed with the opened water-soluble fibers twice, with bagging performed during the mixing process. After mixing, the fibers proceed directly to the carding process. The moisture regain during the carding process is controlled between 10% and 19%. For the carding of blended fibers, the speed ratio between the cylinder and the work roll is between 360 / 2.5 and 180 / 2.5, the speed ratio between the cylinder and the doffer is between 360 / 21 and 340 / 17, the distance between the cylinder and the work roll is between 1.3 mm and 1.6 mm, and the distance between the cylinder and the doffer is between 0.2 mm and 0.65 mm. For the spinning of blended fibers, the draft ratio is between 1.05 and 1. The yarn twist is between 0.45 and 300T / M to 500T / M, with a twist direction of "Z" and a spindle speed between 6500 rpm and 7000 rpm. For blended fibers, a winding and twisting process is performed, with the spinning speed during winding between 400m / min and 650m / min, and the spinning speed during doubling between 5500 rpm and 6500 rpm, with a twist between 200T / M and 400T / M and a twist direction of "S".

[0046] Step D: Using a fancy twisting machine, select an antibacterial functional yarn as the core yarn and several water-soluble blended yarns as the fixing yarn to make an antibacterial composite yarn; wherein the hollow spindle twist is 400 T / M~700 T / M, twist direction "Z", the external twist is 200 T / M~400 T / M, twist direction "S", the overfeed ratio is 2, the draft ratio is 5 times to 20 times, and the core yarn tension is 0.5%~5.5%.

[0047] Step E: Wash the antibacterial composite yarn with water to dissolve the water-soluble fibers within it; the washing temperature should be 40℃ or higher. Step G: Dry the antibacterial composite yarn.

[0048] Example 6: A method for preparing an antibacterial and antiviral yarn with a core-shell structure, comprising the following steps: Step A: Preparing an antibacterial and antiviral shell precursor, by weight, 1.2 parts of nano-inorganic metal oxide powder, 6.0 parts of nano-inorganic oxide modified material, 3.0 parts of natural Chinese herbal medicine preparation, 38.95 parts of chitin protein, and 60 parts of deionized water. In a reaction vessel, the mixture is stirred at 3000 rpm and reacted at 90°C for 3 hours. The nano-inorganic metal oxide powder is aluminum oxide with a particle size of 42.8 nanometers; the nano-inorganic oxide modified material is anionic dimethylsiloxane activator. The natural Chinese herbal medicine preparation is a mixture of Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria in a weight ratio of 30:20:30:20, processed into an ultrafine powder larger than 220 mesh.

[0049] Step B: By weight, 50 parts of antibacterial and antiviral shell precursor are mixed with 50 parts of softened water to form a shell fiber treatment solution. This solution is then used to treat textile fibers to form antibacterial functional fibers, specifically nylon yarn. The nylon yarn is continuously processed in a sizing machine, with the liquid extraction rate controlled at 80%. The temperature is adjusted to 125℃ in the final drying stage, while the rest of the process follows conventional sizing procedures. The final product is antibacterial functional yarn.

[0050] Step C: By weight percentage, select 85% cashmere and 15% water-soluble fiber to form a blended fiber, and then make the water-soluble fiber into a water-soluble blended yarn; the water-soluble fiber is polyvinyl alcohol fiber. For blended fibers, the process involves first mixing and layering cashmere twice, then adding a blending agent and beating once more. The water-soluble fibers are then opened separately. Next, the pre-bleached cashmere is layered and mixed with the opened water-soluble fibers twice, with bagging performed during the mixing process. After mixing, the fibers proceed directly to the carding process. The moisture regain during the carding process is controlled between 10% and 19%. For the carding of blended fibers, the speed ratio between the cylinder and the work roll is between 360 / 2.5 and 180 / 2.5, the speed ratio between the cylinder and the doffer is between 360 / 21 and 340 / 17, the distance between the cylinder and the work roll is between 1.3 mm and 1.6 mm, and the distance between the cylinder and the doffer is between 0.2 mm and 0.65 mm. For the spinning of blended fibers, the draft ratio is between 1.05 and 1. The yarn twist is between 0.45 and 300T / M to 500T / M, with a twist direction of "Z" and a spindle speed between 6500 rpm and 7000 rpm. For blended fibers, a winding and twisting process is performed, with the spinning speed during winding between 400m / min and 650m / min, and the spinning speed during doubling between 5500 rpm and 6500 rpm, with a twist between 200T / M and 400T / M and a twist direction of "S".

[0051] Step E: Using a fancy twisting machine, select an antibacterial functional yarn as the core yarn and several water-soluble blended yarns as the binding yarn to make an antibacterial composite yarn; wherein the hollow spindle twist is 400 T / M to 700 T / M, twist direction "Z", the external twist is 200 T / M to 400 T / M, twist direction "S", the overfeed ratio is 2, the draft ratio is 5 times to 20 times, and the core yarn tension is 0.5% to 5.5%.

[0052] Step F: Wash the antibacterial composite yarn with water to dissolve the water-soluble fibers within it; the washing temperature should be 40℃ or higher. Step G: Dry the antibacterial composite yarn.

Claims

1. A method for preparing antibacterial and antiviral yarn with a core-shell structure, characterized in that, Includes the following steps: Step A: Prepare the antibacterial and antiviral shell precursor. By weight, place 0.05-1.2 parts of nano-inorganic metal oxide powder, 0.5-6.0 parts of organosilicon surfactant, 0.5-3.0 parts of natural Chinese herbal medicine preparation, 29.8-38.95 parts of chitin protein, and 50-70 parts of deionized water in a reaction vessel and react at 80-90°C with stirring at 800-3000 rpm for 1.5-3 hours. The nano-inorganic metal oxide powder is aluminum oxide with a particle size of 15.3-91.6 nm. The organosilicon surfactant includes cationic, anionic, nonionic, or amphoteric dimethylsiloxane series surfactants. The natural Chinese herbal medicine preparation is a mixture of powders larger than 200 mesh from Coptis chinensis, Isatis indigotica, Sophora flavescens, and Isatis tinctoria. Step B: By weight, 40 to 60 parts of the antibacterial and antiviral shell precursor are mixed with 40 to 60 parts of softened water to form a shell fiber treatment solution. Textile fibers are treated with the shell fiber treatment solution to form antibacterial functional fibers. Step C: The antibacterial functional fibers are made into antibacterial functional yarn; Step D: By weight percentage, 85% cashmere and 15% polyvinyl alcohol fiber are mixed to form a blended fiber, which is then processed by blending, combing, spinning, winding and twisting to form a water-soluble blended yarn. Step E: Using a fancy twisting machine, with the antibacterial functional yarn as the core yarn and several strands of the water-soluble blended yarn as the binding yarn, an antibacterial composite yarn is produced; wherein, the hollow spindle twist is 400 T / M to 700 T / M with a twist direction of Z, the external twist is 200 T / M to 400 T / M with a twist direction of S, the overfeed ratio is 2, the draft ratio is 5 to 20 times, and the core yarn tension is 0.5% to 5.5%; Step F: Wash the antibacterial composite yarn at 40°C or above to dissolve the polyvinyl alcohol fibers in the yarn, retain the cashmere fibers in the yarn, and create gaps in the yarn; after washing, treat the antibacterial composite yarn with the shell fiber treatment solution by spraying or impregnation. Step G: Dry the antibacterial composite yarn treated in step F.

2. The method for preparing antibacterial and antiviral yarn with a core-shell structure according to claim 1, characterized in that, In step B, the mass ratio of the shell fiber treatment solution to the textile fiber is 1:1 to 1:10 in the dyeing machine, and the mixture is placed in a water bath at 80℃ to 90℃ for 1.5 to 3 hours. After the water bath, the mixture is dehydrated and then dried using a hot air dryer or a drum dryer. During the drying process, the temperature of the last section is controlled at 120℃ to 130℃.

3. The method for preparing antibacterial and antiviral yarn with a core-shell structure according to claim 1, characterized in that, In step D, the cashmere is mixed, layered, and beaten twice, then mixed once more after adding a wool-retaining agent. Polyvinyl alcohol (PVA) fibers are opened separately. The cashmere after being sealed in a storage chamber is layered and beaten twice with the opened PVA fibers, then bagged. After mixing, the mixture enters the carding process, with the moisture regain controlled at 10%–19%. During carding, the speed ratio between the cylinder and the work roller is 360 / 2.5–180 / 2.5, the speed ratio between the cylinder and the doffer is 360 / 21–340 / 17, the distance between the cylinder and the work roller is 1.3 mm–1.6 mm, and the distance between the cylinder and the doffer is 0.2 mm–0.65 mm. During spinning, the draft ratio is 1.05–1.45, the single yarn twist is 300 T / M–500 T / M, the twist direction is Z, and the spindle speed is 6500 rpm–7000 rpm. During winding and twisting, the winding speed is 400 rpm. The speed of the machine is 5500 rpm to 650 m / min, the twisting speed is 5500 rpm to 6500 rpm, the twist is 200 T / M to 400 T / M, and the twist direction is S.

Citation Information

Patent Citations

  • Preparation method of anti-wrinkling and antibacterial compound yarn strip

    CN102978768A

  • Manufacturing method of antibacterial and antiviral cashmere viscose blended yarn

    CN111926429A

  • Copper yarn, fabric using copper yarn, and copper fabric manufacturing method

    JP2022143719A