Polymer compound and resin composition containing the same

By reacting a random copolymer resin composition of hydroxyphenyl (meth)acrylate and styrene with a free radical initiator in high-frequency circuit substrate applications, the problem of insufficient dielectric properties of existing phenoxy resins is solved. It achieves low dielectric properties and excellent bonding properties and heat resistance, making it suitable for high-frequency circuit substrates.

CN115768805BActive Publication Date: 2024-10-01NIPPON KAYAKU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180044708.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-07-09
Filing Date
2021-06-30
Publication Date
2024-10-01
Estimated Expiration
2041-06-30

AI Technical Summary

Technical Problem

The dielectric properties of existing phenoxy resins in high-frequency circuit substrate applications cannot meet the requirements for low dielectric properties, and their heat resistance and bonding properties are insufficient.

Method used

A polymer compound resin composition containing a specific structure is used to react with a free radical initiator to form a cured product with excellent dielectric properties, bonding properties and heat resistance. The polymer compound is a random copolymer of hydroxyphenyl (meth)acrylate and styrene, synthesized using a free radical polymerization method, and a maleimide compound is added to improve reactivity.

Benefits of technology

A polymer compound that achieves low dielectric constant and low dielectric loss tangent has excellent dielectric properties, bonding properties and heat resistance. It is suitable for bonding low-roughness copper foils and meets the needs of high-frequency circuit substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115768805B_ABST
    Figure CN115768805B_ABST
Patent Text Reader

Abstract

The present invention relates to a polymer compound represented by the following formula (1), which has sufficient flexibility to be formed into a film, has high adhesion to low-roughness copper foil, and has low dielectric constant and dielectric loss tangent (wherein, R 1 and R 2 Each independently represents a hydrogen atom or a methyl group. m and n are average values ​​of the number of repeating units and each independently represents a real number in the range of 1 to 2,000). #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer compound which can be easily formed into a film by casting a solution into a substrate, can undergo a heat or light curing reaction by using it in combination with a radical initiator, and has excellent dielectric properties and bonding properties. Background Art

[0002] Phenoxy resin is a polymer compound with a very large molecular weight obtained by polymerizing a bifunctional epoxy resin and a bifunctional phenol compound. Since a general epoxy resin composition or a radical polymerizable composition can be formed into a film shape by adding the phenoxy resin, it is used as an important component of a film adhesive in a wide range of fields, especially in the interlayer insulating layer of a printed circuit board or a copper foil with resin in the electrical / electronic field.

[0003] Although the cured product of the resin composition added with phenoxy resin has excellent bonding and the ability to form a film, it has low heat resistance, and high dielectric constant and dielectric loss tangent (dielectric constant 3.5 and dielectric loss tangent 0.03 at a frequency of 1 GHz), it cannot be used in electronic equipment applications with high signal response speed in recent years. Generally known resins with excellent dielectric properties include high molecular fluorine compounds such as polytetrafluoroethylene (PTFE) (Patent Document 1) and liquid crystal polymers (Patent Document 2), but these resins have extremely low compatibility with other resins and insufficient bonding. Patent document 3 describes a curable polymer compound obtained by esterifying aliphatic hydroxyl groups in a random copolymer of less than 70 wt % of a monomer having one ethylenically unsaturated group and more than 30 wt % of a (meth)acrylate having one or more aliphatic hydroxyl groups with a monomer having one or more ethylenically unsaturated groups and one carboxyl group. However, when the inventors conducted additional experiments, they found that the dielectric loss tangent of the cured polymer compound obtained from the structural formula of the same document was about 0.005 at 10 GHz, which could not fully meet the low dielectric properties sought for current high-frequency circuit substrate applications.

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2005-001274

[0007] [Patent Document 2] Japanese Patent Application Publication No. 2014-060449

[0008] [Patent document 3] Japanese Patent Application Publication No. 10-017812. Summary of the invention

[0009] [Problems to be solved by the invention]

[0010] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a curable polymer compound having sufficient flexibility to be formed into a film, high adhesion to a low-roughness copper foil, and low dielectric constant and dielectric loss tangent.

[0011] [Methods to solve the problem]

[0012] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by using a resin composition containing a polymer compound of a specific structure, thereby completing the present invention.

[0013] That is, the present invention relates to the following inventions:

[0014] (1) A polymer compound represented by the following formula (1),

[0015]

[0016] (wherein, R1 and R2 each independently represent a hydrogen atom or a methyl group. m and n are average values ​​of the number of repeating units and each independently represent a real number in the range of 1 to 2,000);

[0017] (2) A resin composition comprising the polymer compound described in the above item (1) and a free radical initiator;

[0018] (3) The resin composition as described in the above item (2), further comprising a radical reactive monomer having two or more functional groups in one molecule;

[0019] (4) The resin composition according to the above item (3), wherein the radical reactive monomer is a maleimide compound;

[0020] (5) A film adhesive comprising the resin composition described in any one of (2) to (4); and

[0021] (6) A cured product, which is the resin composition according to any one of the above items (2) to (4) or the film adhesive according to the above item (5).

[0022] [Effects of the Invention]

[0023] The polymer compound and the resin composition containing the polymer compound of the present invention are flexible and can be cured by applying heat or light energy in combination with a free radical initiator. The cured product of the resin composition has excellent dielectric properties, bonding properties, heat resistance and water resistance. DETAILED DESCRIPTION

[0024] Hereinafter, embodiments of the present invention will be described.

[0025] The polymer compound represented by the above formula (1) of the present invention is the following compound: a dehydrochlorinated condensate of a hydroxyl group possessed by a random copolymer of hydroxyphenyl (meth)acrylate and styrene and a chloride group of (meth)acryloyl chloride; or a dehydrated condensate of a hydroxyl group possessed by the aforementioned random copolymer and (meth)acrylic acid.

[0026] First, a random copolymer (hereinafter also referred to as an intermediate copolymer) which is an intermediate raw material of the polymer compound of the present invention will be described.

[0027] The hydroxyphenyl (meth)acrylate which is a raw material of the intermediate copolymer is not particularly limited. Specific examples of the hydroxyphenyl (meth)acrylate include 4-hydroxyphenyl methacrylate, 2-hydroxyphenyl methacrylate, 3-hydroxyphenyl methacrylate, 4-hydroxyphenyl acrylate, 2-hydroxyphenyl acrylate, and 3-hydroxyphenyl acrylate, and 4-hydroxyphenyl methacrylate is preferred.

[0028] In addition, in this specification, the description of "(meth)acrylate" means both "acrylate and methacrylate".

[0029] The following formula (2) is a structural formula of a random copolymer of hydroxyphenyl (meth)acrylate and styrene, and R1, m and n in formula (2) have the same meanings as R1, m and n in formula (1). That is, the polymer compound represented by formula (1) of the present invention (polymer compound having a structure represented by formula (1)) is a polymer compound using the intermediate copolymer represented by the following formula (2) as an intermediate raw material.

[0030]

[0031] The copolymerization method of hydroxyphenyl (meth)acrylate and styrene is not particularly limited as long as it is a publicly known method, and examples thereof include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization.

[0032] Solvents that can be used in solution polymerization include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentane, cyclohexanone, propylene glycol monomethyl ether acetate, N-methylpyrrolidone, N,N-dimethylformamide, and γ-butyrolactone. Water and a surfactant are usually used in emulsion polymerization and suspension polymerization to carry out copolymerization in a state where the raw material components are emulsified or suspended in water.

[0033] The copolymerization reaction of (meth) hydroxyphenyl acrylate and styrene can be any one of free radical polymerization, cationic polymerization and anionic polymerization. In the case of free radical polymerization, a free radical polymerization initiator is preferably used. Specific examples of free radical polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis[2-(2-imidazoline-2-yl)propane]dihydrochloride, hydrogen peroxide, di(tert-butyl)peroxide, dicumyl peroxide, and benzoyl peroxide.

[0034] The amount of the free radical polymerization initiator is usually 0.001 to 5 parts by mass relative to a total of 100 parts by mass of the raw material components of the intermediate copolymer. The polymerization temperature is usually 50 to 250° C., preferably 60 to 200° C., and the polymerization time is usually 0.5 to 30 hours, preferably 1 to 20 hours. In order to prevent polymerization inhibition caused by oxygen in the air, the free radical polymerization reaction is preferably carried out under a nitrogen environment.

[0035] If it is cationic polymerization, it is preferred to use a cationic polymerization initiator. The specific example of the cationic polymerization initiator can be a mineral acid such as sulfuric acid and hydrochloric acid, CF3COOH and CCl3COOH and other organic acids, CF3SO3H and HClO4 and other superacids. And, if it is anionic polymerization, it is preferred to use anionic polymerization initiators. The specific example of anionic polymerization initiators can be butyl lithium, naphthalene sodium complex, alkali metal, alkyl lithium compound, sodium amide, Grignard reagent (Grignard reagent) and lithium alkoxide etc. However, the ionic initiator used in cationic polymerization or anionic polymerization, because it still remains in the intermediate copolymer after the polymerization reaction, has a concern of causing adverse effects on dielectric properties and insulation, so the synthesis of the intermediate copolymer that becomes the intermediate raw material of the polymer compound of the present invention is preferably carried out by free radical polymerization.

[0036] The amount of the cationic polymerization initiator or anionic polymerization initiator is usually 0.01 to 5 parts by mass relative to 100 parts by mass of the total raw material components of the intermediate copolymer. The polymerization temperature is usually 40 to 150° C., preferably 50 to 120° C., and the polymerization time is usually 0.5 to 20 hours, preferably 1 to 15 hours.

[0037] The number average molecular weight of the intermediate copolymer of the polymer compound of the present invention is usually 3,000 to 300,000, preferably 5,000 to 200,000.

[0038] In order to obtain the intermediate copolymer with a predetermined number average molecular weight m and n, it is preferred to adjust the amount of the initiator used when synthesizing the intermediate copolymer to an appropriate amount. The amount of the initiator required to obtain the intermediate copolymer with a predetermined number average molecular weight m and n varies depending on the type of the (meth)acrylate having a phenolic hydroxyl group and the amount of the (meth)acrylate having a hydroxyl group and styrene used in the copolymerization reaction, so it is impossible to generalize. However, it is generally known that if the amount of the initiator is reduced, an intermediate copolymer with a large molecular weight can be obtained. Therefore, it is sufficient to select the initiator blending amount within the above-mentioned blending amount range to obtain the intermediate copolymer with the desired molecular weight.

[0039] The ratio of hydroxyphenyl (meth)acrylate to styrene used in the synthesis of the intermediate copolymer as the intermediate raw material of the polymer compound of the present invention is not particularly limited, and the amount (mass) of styrene used is generally 4 to 99.7 times the mass of hydroxyphenyl (meth)acrylate, preferably 4.5 to 99.5 times. By setting the ratio of the raw materials of the intermediate copolymer to the aforementioned range, the polymer compound of the present invention can be obtained, the cured product of which exhibits excellent dielectric properties (low dielectric constant and low dielectric loss tangent).

[0040] The polymer compound of the present invention is obtained by a dehydrochlorination reaction of a phenolic hydroxyl group of the intermediate copolymer (the hydroxyl group is a hydroxyl group of hydroxyphenyl (meth)acrylate which is a raw material) and a chloride group of (meth)acryloyl chloride, or a dehydration condensation reaction of a phenolic hydroxyl group of the intermediate copolymer and (meth)acrylic acid.

[0041] The ratio of the intermediate copolymer and (meth)acryloyl chloride or (meth)acrylic acid used in synthesizing the polymer compound of the present invention is not particularly limited. However, when (meth)acryloyl chloride or (meth)acrylic acid is in excess or deficiency relative to the hydroxyl groups of the intermediate copolymer, the (meth)acryloyl chloride or (meth)acrylic acid remaining in the polymer compound without reacting or the hydroxyl groups remaining without reacting with (meth)acryloyl chloride or methacrylic acid may adversely affect various properties of the cured product. Therefore, it is preferred to use (meth)acryloyl chloride or (meth)acrylic acid in an amount equivalent to the hydroxyl groups of the intermediate copolymer.

[0042] The reaction of the intermediate copolymer and (meth) acryloyl chloride is carried out by adding (meth) acryloyl chloride to the organic solvent solution of the intermediate copolymer under stirring and reacting it. Here, the organic solvent that can be used is an organic solvent that can dissolve the intermediate copolymer and (meth) acryloyl chloride, and is not particularly limited. When synthesizing the intermediate copolymer in a solvent, the intermediate copolymer solution after the polymerization reaction can be directly used. The concentration of the intermediate copolymer solution for reacting with (meth) acryloyl chloride is generally 10 to 90% by mass, preferably 20 to 80% by mass. Moreover, the reaction temperature is generally 30 to 120°C, preferably 40 to 110°C, and the reaction time is generally 0.5 to 4 hours, preferably 1 to 3 hours.

[0043] Since the reaction between the intermediate copolymer and (meth)acryloyl chloride is a dehydrochlorination reaction, in order to capture the generated hydrochloric acid and further promote the reaction, it is preferred to pre-add a tertiary amine such as triethylamine or pyridine to the reaction solution. The amount of the tertiary amine used is preferably equimolar to 4 times the molar amount of (meth)acryloyl chloride, and more preferably equimolar to 3 times the molar amount. Since the hydrochloric acid generated during the reaction is precipitated in the form of amine hydrochloride, it can be removed by filtering after the reaction. In addition, the excess tertiary amine can be distilled out of the system under heating and reduced pressure after filtering.

[0044] The reaction of the intermediate copolymer and (meth)acrylic acid may be, for example, an esterification reaction known in the art, such as a method of heating and stirring the intermediate copolymer and (meth)acrylic acid in the presence of a catalyst. Since the reaction of the intermediate copolymer and (meth)acrylic acid is a dehydration reaction, it is preferably carried out while removing water from the reaction system by azeotropic distillation. Therefore, it is preferred to use a solvent such as toluene, xylene, ethyl acetate, butyl acetate, and methyl isobutyl ketone that is completely immiscible with water for the reaction. The amount of the solvent used is preferably an amount that makes the concentration of the raw material component of the polymer compound 20 to 80% by mass.

[0045] The catalyst used in the esterification reaction may be an acidic catalyst such as sulfuric acid, methanesulfonic acid, and p-toluenesulfonic acid, and the amount used is preferably 0.1 to 5% by mass relative to the total mass of the raw material components of the polymer compound and the solvent used in the reaction. The reaction temperature is usually 50 to 150° C., preferably 60 to 140° C., and the reaction time is usually 0.5 to 4 hours, preferably 1 to 3 hours.

[0046] In addition, in order to prevent the polymerization reaction of the (meth)acryloyl groups in the polymer compound of the present invention during storage, it is preferred to add a small amount of polymerization inhibitor to the polymer compound solution after the synthesis reaction. Specific examples of the polymerization inhibitor include hydroquinone, p-methoxyphenol, methylhydroquinone, di-tert-butylhydroxytoluene, tert-butylhydroquinone, 2-tert-butyl-1,4-benzoquinone, 1,4-benzoquinone, 1,1-diphenyl-2-trinitrophenylhydrazine radical (1,1-diphenyl-2-picrylhydrazyl radical), 6-tert-butyl-2,4-xylenol, 4-tert-butylcatechol, 2,6-di-tert-butylphenol, 2,6-di-tert-butyl-p-cresol and phenothiazine.

[0047] The number average molecular weight of the polymer compound of the present invention thus obtained is preferably in the range of 11,000 to 300,000, more preferably 15,000 to 200,000. When the molecular weight is smaller than the above range, the bonding property to the low roughness copper foil may be reduced, and when the molecular weight is larger than the above range, the viscosity may be increased, making coating difficult.

[0048] In addition, the molecular weight in this specification refers to the value calculated based on the measurement result of GPC and converted into polystyrene.

[0049] The resin composition of the present invention contains the polymer compound of the present invention and a radical initiator.

[0050] As the free radical initiator, a thermal free radical initiator and / or a photo free radical initiator can be used. Preferred thermal radical initiators include peroxides such as benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, di-tert-butyl peroxide, tert-butylcumene peroxide, α,α-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisophenylpropyl peroxide, di(tert-butylperoxyisophthalate), tert-Butylperoxybenzoate, 2,2-bis(tert-butylperoxy)butane, 2,2-bis(tert-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilylperoxide.

[0051] Preferred examples of photoradical initiators include: benzoin and its alkyl ethers such as benzoin, benzoin methyl ether, and benzoin ethyl ether; acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone; anthraquinones such as 2-methylanthraquinone, 2-amylanthraquinone, 2-tert-butylanthraquinone, and 1-chloroanthraquinone; thioxanthones such as 2,4-dimethylthioxanthone, 2,4-diisopropylthioxanthone, and 2-chlorothioxanthone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; diphenyl ketones such as diphenyl ketone; 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propane-1-one or 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1; acylphosphine oxides (acylphosphine oxides and xanthone.

[0052] The content of the radical initiator in the resin composition of the present invention is usually 0.1 to 10 parts by mass, preferably 0.1 to 8 parts by mass, based on 100 parts by mass of the total of the polymer compound and the resin components such as the radical reactive monomer which is an optional component described below.

[0053] The resin composition of the present invention may further include a free radical reactive monomer. By using a free radical reactive monomer, the reactivity of the resin composition of the present invention or the heat resistance of the cured product can be improved. The free radical reactive monomer is preferably a monomer having two or more functional groups, and specific examples thereof include ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, neopentyl glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, glycerol dimethacrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, bisphenol A ethylene oxide adduct methacrylate, trimethylolpropane trimethacrylate, tricyclodecane dimethacrylate, etc. Methanol dimethacrylate, glycerol dimethacrylate, trimethylolpropane trimethacrylate, ethoxylated isocyanuric acid triacrylate, ε-caprolactone modified 3-(2-acryloyloxyethyl) isocyanurate, pentaerythritol triacrylate, di-trimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, pentaerythritol tetraacrylate, dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, divinyl isophthalate, N-phenyl-maleimide, N-phenyl-methylmaleimide imide, N-phenyl-chloromaleimide, N-p-chlorophenyl-maleimide, N-p-methoxyphenyl-maleimide, N-p-methylphenyl-maleimide, N-p-nitrophenyl-maleimide, N-p-phenoxyphenyl-maleimide, N-p-phenylaminophenyl-maleimide, N-p-phenoxycarbonylphenyl-maleimide, 1-maleimide-4-acetoxysuccinimide-benzene, 4-maleimide-4'-acetoxysuccinimide-diphenylmethane, 4-maleimide-4'-acetoxysuccinimide-diphenyl ether, 4-maleimide Maleimide-4'-acetamide-diphenyl ether, 2-maleimide-6-acetamide-pyridine, 4-maleimide-4'-acetamide-diphenylmethane and N-p-phenylcarbonylphenyl-maleimide N-ethylmaleimide, N-2,6-xylylmaleimide, N-cyclohexylmaleimide, N-2,3-xylylmaleimide, xylylmaleimide, 2,6-xylylmaleimide and 4,4'-bismaleimide diphenylmethane, etc., preferably a compound having a maleimide group as a functional group (i.e., a maleimide compound).

[0054] These radical reactive monomers may be used alone or in combination of two or more.

[0055] The resin composition of the present invention may contain an organic solvent. Specific examples of organic solvents include aromatic solvents such as toluene and xylene, ether solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate and propylene glycol monobutyl ether, methyl ethyl ketone, methyl isobutyl ketone, ketone solvents such as cyclopentane and cyclohexanone, lactones such as gamma-butyrolactone and gamma-valerolactone, N-methylpyrrolidone (Methylpyrrolidone) (NMP), N, N-dimethylformamide (DMF), N, N-dimethylacetamide and N, N-dimethylimidazolidinone, sulfones such as sulfone (tetramethylene sulfone), etc. Relative to the total amount of the resin composition, the content of the organic solvent in the resin composition of the present invention is usually less than 90% by mass, preferably 30 to 80% by mass.

[0056] In order to improve storage stability, the resin composition of the present invention may be used in combination with a polymerization inhibitor. The polymerization inhibitor that can be used in combination is not particularly limited as long as it is a generally known polymerization inhibitor, and examples thereof include quinones such as hydroquinone, methylhydroquinone, p-benzoquinone, chloranil, and trimethylquinone, or aromatic diols, di-tert-butylhydroxytoluene, and the like.

[0057] In the resin composition of the present invention, for the purpose of imparting desired performance corresponding to its use, a filler or additive in an amount within a range that does not impair the original performance can be formulated. The filler can be fibrous or powdery, and examples thereof include silica, carbon black, alumina, talc, mica, glass beads, and hollow glass spheres.

[0058] Flame retardant compounds, additives, etc. may also be added to the resin composition of the present invention. As long as these are generally used flame retardant compounds, additives, etc., there is no particular limitation. For example, flame retardant compounds may include bromine compounds such as 4,4-dibromobiphenyl, phosphate esters, melamine phosphate, phosphorus-containing epoxy resins, nitrogen compounds such as melamine or benzoguanamine, compounds containing oxazine rings, silicon compounds, etc. Additives may be appropriately combined to use ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, dispersants, levelers, glossing agents, etc. according to the desired requirements.

[0059] The resin composition of the present invention can be applied or impregnated on various substrates for use. For example, when a thermal free radical initiator is used, it can be applied on a PET film as an interlayer insulating layer of a multilayer printed substrate, applied on a polyimide film as a protective film (coverley), or applied on a copper foil and dried as a copper foil with resin. In addition, it can also be used as a prepreg of a printed circuit board or CFRP by impregnating it in glass cloth or glass paper, carbon fiber, various non-woven fabrics, etc. In addition, it can be used as various resists by using a photo radical initiator.

[0060] The interlayer insulating layer, protective film, copper foil with resin, prepreg, etc. of the present invention can be formed into a cured product by heating and pressing with a hot press or the like.

[0061] [Example]

[0062] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples. In addition, the present invention is not limited to these Examples. In addition, "parts" in the Examples refer to parts by mass.

[0063] Example 1 (Synthesis of the polymer compound of the present invention)

[0064] (Step 1) Synthesis of an intermediate copolymer (intermediate copolymer 1) represented by the following formula (3):

[0065] In a flask equipped with a thermometer, a cooling tube, a nitrogen inlet tube, and a stirrer, 38.5 parts of styrene, 1.5 parts of 4-hydroxyphenyl methacrylate, 0.4 parts of benzoyl peroxide, and 10 parts of propylene glycol monomethyl ether acetate (PGMEA) were added, and reacted at 120 to 130° C. for 5 hours under a nitrogen atmosphere to obtain a PGMEA solution of an intermediate copolymer 1 represented by the following formula (3). A portion of the above PGMEA solution was heated under reduced pressure, and the yield of the intermediate copolymer 1 calculated as the solid content by taking into account the dry mass after removing the solvent and unreacted styrene was 34.2 parts and the unreacted styrene was 5.8 parts. The intermediate copolymer 1 obtained was a copolymer of 32.7 parts of styrene and 1.5 parts of 4-hydroxyphenyl methacrylate. The number average molecular weight of the sample used to measure the above dry mass was 38,000, and the weight average molecular weight was 161,000. From the copolymerization ratio and number average molecular weight of styrene and 4-hydroxyphenyl methacrylate, the value of n in formula (3) was calculated to be 361 and the value of m was 9.

[0066]

[0067] (Step 2) Synthesis of the polymer compound of the present invention represented by the following formula (4) (polymer compound 1)

[0068] From the PGMEA solution of the intermediate copolymer 1 obtained in step 1, unreacted styrene is distilled off together with PGMEA under heating and reduced pressure, and then PGMEA is added to obtain 138 parts of a 25% by mass solution of the intermediate copolymer 1. 5 parts of triethylamine are added to the solution, and 0.88 parts of methacryloyl chloride are added at 60°C under stirring and reacted for 1 hour. The reaction solution is filtered under pressure with a filter paper having a compensation particle size of 1 micron to remove triethylamine hydrochloride, and excess triethylamine and PGMEA are distilled off from the filtrate by a rotary evaporator. The amount of PGMEA is adjusted to obtain 139 parts of a solution containing 25% by mass of the polymer compound of the present invention (polymer compound 1) represented by the following formula (4). The number average molecular weight of the obtained polymer compound 1 is 40,000, and the weight average molecular weight is 164,000.

[0069]

[0070] Comparative Example 1 (Synthesis of a comparative polymer compound represented by the following formula (6))

[0071] (Step 3) Synthesis of an intermediate copolymer (intermediate copolymer 2) represented by the following formula (5):

[0072] According to step 1, except that 1.5 parts of 4-hydroxyphenyl methacrylate was replaced by 1.5 parts of 2-hydroxyethyl methacrylate, a PGMEA solution of an intermediate copolymer 2 represented by the following formula (5) was obtained. A portion of the aforementioned PGMEA solution was heated under reduced pressure. If the yield of the intermediate copolymer 2 calculated by taking the dry mass after removing the solvent and unreacted styrene as the solid content was 35.6 parts and the unreacted styrene was 4.4 parts, the intermediate copolymer obtained was a copolymer of 34.1 parts of styrene and 1.5 parts of 2-hydroxyethyl methacrylate. In addition, the number average molecular weight of the sample used to measure the aforementioned dry mass was 45,000, and the weight average molecular weight was 177,000. From the copolymerization ratio and number average molecular weight of styrene and 2-hydroxyethyl methacrylate, the value of n in formula (5) was calculated to be 414, and the value of m was 14.

[0073]

[0074] (Step 4) Synthesis of a comparative polymer compound (polymer compound 2) represented by the following formula (6):

[0075] Except that the intermediate copolymer 1 was changed to the intermediate copolymer 2 obtained in step 3 and the amount of methacryloyl chloride used was changed from 0.88 parts to 1.20 parts, 145 parts of a solution containing 25% by mass of a comparative polymer compound (polymer compound 2) represented by the following formula (6) was obtained according to step 2. The number average molecular weight of the obtained polymer compound 2 was 47,000 and the weight average molecular weight was 182,000.

[0076]

[0077] Example 2 (Preparation of the resin composition of the present invention)

[0078] To 10 parts of the PGMEA solution of the polymer compound 1 of the present invention obtained in Example 1, 0.05 parts of diisophenylpropyl peroxide was added as a radical initiator and the mixture was uniformly mixed to obtain a resin composition 1 of the present invention.

[0079] Comparative Example 2 (Preparation of a comparative resin composition)

[0080] A comparative example resin composition 1 was obtained according to Example 2 except that the PGMEA solution of the polymer compound 1 of the present invention was changed to the PGMEA solution of the comparative example polymer compound 1 obtained in Comparative Example 1.

[0081] (Evaluation of Dielectric Properties of Cured Resin Composition)

[0082] Using an applicator, the resin composition 1 of the present invention and the comparative example resin composition 1 obtained in Example 2 and Comparative Example 2 were respectively applied to the mirror surface of a copper foil having a thickness of 18 μm at a thickness of 280 μm, and heated at 90°C for 10 minutes to dry the solvent, thereby obtaining a copper foil having a film adhesive composed of the resin composition. The film adhesive on the copper foil obtained above was heated and hardened at 180°C for 1 hour in a vacuum oven, and then immersed in an etching solution and the copper foil was removed, thereby obtaining a cured film adhesive having a thickness of 70 μm that can be used as a film. Using Networkanalyzer 8719ET (manufactured by Agilent Technologies), the dielectric constant and dielectric loss tangent of the cured product obtained above at 10 GHz were measured by the cavity resonance method. The results are shown in Table 1.

[0083] (Evaluation of bonding strength of cured product of resin composition)

[0084] Using an applicator, the resin composition 1 of the present invention and the comparative example resin composition 1 obtained in Example 2 and Comparative Example 2 were applied to the rough surface of a 12 μm thick high-frequency low-roughness copper foil (CF-T4X-SV: manufactured by Fukuda Metal Foil Co., Ltd.) at a thickness of 50 μm, respectively, and heated at 90°C for 10 minutes to dry the solvent, thereby obtaining a copper foil having a film-like adhesive composed of the resin composition. On the adhesive surface of the copper foil with resin obtained above, the rough surface of the same copper foil as above was overlapped, and after heating and curing at a pressure of 3 MPa for 1 hour in a vacuum press, the 90° peel strength (bonding strength) between the copper foils was measured using AUTOGRAPH AGX-50 (manufactured by Shimadzu Corporation). The results are shown in Table 1.

[0085] [Table 1]

[0086] Table 1: Evaluation results of cured products of resin compositions

[0087]

[0088]

[0089] As described above, the polymer compound of the present invention forms a flexible film when cured using a radical initiator, and further exhibits excellent dielectric properties and bonding properties.

Claims

1. A polymer compound represented by the following formula (1), having a number average molecular weight of 11,000 to 300,000, In the formula, R1 and R2 each independently represent a hydrogen atom or a methyl group; m and n are average values ​​of the number of repeating units, and each independently represent a real number in the range of 1 to 2,000. 2 . A resin composition comprising the polymer compound according to claim 1 and a free radical initiator. 3 . The resin composition according to claim 2 , further comprising a radical reactive monomer having two or more functional groups in one molecule.

4. The resin composition according to claim 3, wherein The free radical reactive monomer is a maleimide compound. 5 . A film adhesive comprising the resin composition according to claim 2 . 6 . A cured product, which is a cured product of the resin composition according to claim 2 or the film adhesive according to claim 5 .