A kind of graphene oxide composite hydrogel and preparation method thereof

The cross-linked structure and π-π are formed by introducing polyethylene glycol-containing hyperbranched polyester and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) into graphene oxide. Conjugation improves the mechanical properties and heavy metal adsorption capacity of graphene oxide composite hydrogel, solves the problem of insufficient mechanical properties of graphene oxide materials, and achieves the effect of efficient adsorption of heavy metals.

CN115779808BActive Publication Date: 2024-10-08SHEN ZHEN WAN ZHI DA QI YE GUAN LI YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211335256.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-10-08
Estimated Expiration
2042-10-28

Smart Images

  • Figure BDA0003915134460000081
    Figure BDA0003915134460000081
Patent Text Reader

Abstract

The invention discloses a graphene oxide composite hydrogel and a preparation method thereof. The graphene oxide composite hydrogel is polymerized by graphene oxide, a hyperbranched polyester copolymer containing polyethylene glycol, and poly(trans-4-carbonyl-4-(thiophene-2-yl)but-2-enoic acid) in a weight ratio of 1:0.5-0.8:0.2-0.5. The graphene oxide composite hydrogel introduces the hyperbranched polyester copolymer containing polyethylene glycol and the poly(trans-4-carbonyl-4-(thiophene-2-yl)but-2-enoic acid) into the molecular structure of graphene oxide, effectively improves the mechanical properties of graphene oxide, and obtains the graphene oxide composite hydrogel with good adsorption performance for heavy metals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional materials, and in particular relates to a graphene oxide composite hydrogel and a preparation method thereof. Background Art

[0002] Heavy metals refer to metals with a density greater than 4.5 g / cm 3 Heavy metal pollution refers to environmental pollution caused by heavy metals or their compounds. It is mainly caused by human factors such as mining, exhaust gas emissions, sewage irrigation and the use of products with excessive heavy metals. Due to human activities, the content of heavy metals in the environment increases beyond the normal range, directly endangering human health and causing environmental quality deterioration.

[0003] At present, many methods for treating heavy metals have been developed, such as traditional chemical precipitation, chelation flocculation, ferrite, ion exchange, evaporation concentration, adsorption, membrane separation and electrochemical methods. Compared with other treatment methods, adsorption has better practicality and broader application prospects due to its wide application range, simple treatment process, wide source of raw materials, low cost and good treatment effect. The selection of adsorbent in adsorption is crucial.

[0004] Polymer hydrogel can be used as an adsorbent for heavy metal ions. It is a moderately cross-linked polymer network system that contains abundant hydrophilic groups and can absorb water and swell in aqueous solution without dissolving in water. The choice of raw materials for hydrogel directly affects its adsorption performance. Graphene oxide has a high specific surface area and a large number of oxygen-containing functional groups on the surface, and has excellent adsorption performance. It is a high-quality material for preparing hydrogel.

[0005] A large number of oxygen-containing groups, including epoxy, hydroxyl, carboxyl, etc., are attached to the surface of graphene oxide. Due to the large number of oxygen-containing functional groups on the surface of graphene oxide, its thickness is also slightly greater than that of graphene. Graphene oxide and graphene also have a two-dimensional planar structure. Due to the addition of oxygen-containing functional groups, graphene oxide exhibits a strong hydrophilicity. It only needs to apply a certain external force (ultrasound, microwave, etc.) to the graphene oxide ink solution to peel off the graphene oxide into a single layer of graphene oxide to obtain a stable dispersion. With the introduction of these oxygen-containing groups, the π bond of graphene is broken, the carbon skeleton structure of graphene is severely damaged, and its mechanical properties are greatly reduced. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a graphene oxide composite hydrogel, which is polymerized by graphene oxide, a hyperbranched polyester copolymer containing polyethylene glycol, and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) at a weight ratio of 1:0.5 to 0.8:0.2 to 0.5. The graphene oxide composite hydrogel introduces a hyperbranched polyester copolymer containing polyethylene glycol and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) into the molecular structure of graphene oxide, effectively improving the mechanical properties of graphene oxide, and obtaining a graphene oxide composite hydrogel with good adsorption performance for heavy metals.

[0007] The object of the present invention is to provide a graphene oxide composite hydrogel, which is prepared by polymerizing graphene oxide, a hyperbranched polyester copolymer containing polyethylene glycol, and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) in a weight ratio of 1:0.5-0.8:0.2-0.5.

[0008] The hydroxyl groups contained in the hyperbranched polyester copolymer containing polyethylene glycol selected in the present scheme can undergo a cross-linking reaction with the hydroxyl groups and carboxyl groups in graphene oxide under the action of diisocyanate to form a cross-linked network structure, thereby improving the mechanical properties of graphene oxide. The hyperbranched polyester runs through the layered structure of graphene oxide, supporting the graphene oxide skeleton, further improving the mechanical properties of the hyperbranched polyester. The chain ends of the hyperbranched polyester contain hydroxyl groups and carboxyl groups, which form hydrogen bonds with the hydroxyl groups and carboxyl groups in graphene oxide, thereby improving the interaction between the hyperbranched polyester and graphene oxide.

[0009] Poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) has an adsorption effect on heavy metals, and there is π-π conjugation between the carbonyl and thiophene groups in the molecular structure, which enhances the adsorption effect of graphene oxide composite hydrogel on heavy metals. The carboxyl group in the molecular structure of poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) can react with the carboxyl and hydroxyl groups in the molecular structure of graphene oxide, and the carboxyl and hydroxyl groups in the molecular structure of the hyperbranched polyester copolymer containing polyethylene glycol through diisocyanate to form a stable cross-linked structure. On the one hand, the formed stable cross-linked structure improves the mechanical properties of graphene oxide, and on the other hand, the hyperbranched polyester copolymer containing polyethylene glycol has low toughness and strength due to the lack of chain entanglement, and the formed stable cross-linked structure enhances the toughness and strength of the hyperbranched polyester copolymer containing polyethylene glycol.

[0010] Preferably, the graphene oxide composite hydrogel is polymerized by graphene oxide, a hyperbranched polyester copolymer containing polyethylene glycol, and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) in a weight ratio of 1:0.6:0.3.

[0011] Preferably, the hyperbranched polyester copolymer containing polyethylene glycol is at least one selected from polyethylene glycol-hyperbranched polyester, polylactic acid-co-glycolic acid-polyethylene glycol-hyperbranched polyester, polylactic acid-polyethylene glycol-hyperbranched polyester, polycaprolactone-polyethylene glycol-hyperbranched polyester.

[0012] More preferably, the polyethylene glycol-containing hyperbranched polyester copolymer is selected from polyethylene glycol-hyperbranched polyester.

[0013] Furthermore, the preparation method of the poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) comprises the following steps:

[0014] Trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid, an initiator and a first solvent are mixed, heated and stirred for 1-3 hours to obtain poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid).

[0015] Preferably, the initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile and lauroyl peroxide.

[0016] More preferably, the initiator is selected from azobisisobutyronitrile.

[0017] Preferably, the first solvent is selected from at least one of ethyl acetate, butanone and acetone.

[0018] More preferably, the first solvent is selected from ethyl acetate.

[0019] Preferably, the molar ratio of the initiator to trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid is 0.001 to 0.004:1.

[0020] More preferably, the molar ratio of the initiator to trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid is 0.003:1.

[0021] Preferably, the heating temperature is 70-80°C.

[0022] Preferably, the heating time is 1 to 3 hours.

[0023] Another object of the present invention is to provide a method for preparing the above-mentioned graphene oxide composite hydrogel, comprising the following steps:

[0024] Step S1. dissolving graphene oxide and a hyperbranched polyester copolymer containing polyethylene glycol in a second solvent according to a weight ratio, adding diisocyanate and a catalyst, heating and stirring, and obtaining a copolymer.

[0025] Step S2. Add diisocyanate and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) to the copolymer obtained in step S1, heat to react, soak the product in deionized water, and freeze-dry to obtain a graphene oxide composite hydrogel.

[0026] Preferably, in step S1, the catalyst is selected from at least one of stannous octoate and dibutyltin dilaurate.

[0027] More preferably, in step S1, the catalyst is selected from dibutyltin dilaurate.

[0028] Preferably, in step S1, the catalyst accounts for 0.5-2% of the total weight of the reaction solution.

[0029] Preferably, the second solvent is selected from at least one of ethyl acetate, butanone and acetone.

[0030] More preferably, the second solvent is selected from ethyl acetate.

[0031] Preferably, in step S1, the weight ratio of the diisocyanate to graphene oxide is 0.5-0.8:1.

[0032] Preferably, in step S1, the heating temperature is 50-70°C.

[0033] Preferably, in step S1, the heating time is 2 to 4 hours.

[0034] Preferably, in step S2, the weight ratio of the diisocyanate to poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) is 0.5-0.8:0.2-0.5.

[0035] Preferably, in step S2, the heating time is 3 to 5 hours.

[0036] Preferably, in step S2, the heating temperature is 50-70°C.

[0037] Preferably, the diisocyanate is at least one selected from the group consisting of xylene diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, p-xylylene diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.

[0038] More preferably, the diisocyanate is selected from isophorone diisocyanate.

[0039] Another object of the present invention is to provide an application of the above-mentioned graphene oxide composite hydrogel in the adsorption of heavy metals. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0041] The hyperbranched polyester copolymer of polyethylene glycol is selected from polyethylene glycol-hyperbranched polyester, polylactic acid-co-glycolic acid-polyethylene glycol-hyperbranched polyester, polylactic acid-polyethylene glycol-hyperbranched polyester, polycaprolactone-polyethylene glycol-hyperbranched polyester, all of which are purchased from Xi'an Ruixi Biotechnology Co., Ltd.

[0042] Graphene oxide was purchased from Changzhou Sixth Element Materials Technology Co., Ltd., with a sheet diameter of 20 to 25 μm.

[0043] Example 1: Preparation of poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid).

[0044] Trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid (10 mmol), azobisisobutyronitrile (0.03 mmol) and ethyl acetate (30 mmol) were mixed, heated and stirred at 70°C for 2 hours to obtain poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid).

[0045] Example 2: Preparation of graphene oxide composite hydrogel.

[0046] Step S1. 1 g of graphene oxide and 0.6 g of polyethylene glycol-hyperbranched polyester were dissolved in 30 g of ethyl acetate according to weight ratio, 0.6 g of isophorone diisocyanate and 0.3 g of dibutyltin dilaurate were added, and the mixture was heated and stirred at 70° C. for 3 hours to obtain a copolymer;

[0047] Step S2. Add 0.6 g of isophorone diisocyanate and 0.3 g of poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) to the copolymer obtained in step S1, heat at 70°C for 4 hours, and after the reaction, soak the product in water, changing the water every 24 hours for 1 week, and then place it in a freeze dryer for freeze drying to obtain graphene oxide composite hydrogel.

[0048] Comparative Example 1: Preparation of graphene oxide composite hydrogel.

[0049] The polyethylene glycol-hyperbranched polyester in Example 2 was replaced by a hyperbranched polyester, and the other steps remained unchanged.

[0050] Comparative Example 2: Preparation of graphene oxide composite hydrogel.

[0051] The polyethylene glycol-hyperbranched polyester in Example 2 was replaced with polyethylene glycol, and the other steps remained unchanged.

[0052] Comparative Example 3: Preparation of graphene oxide composite hydrogel.

[0053] Step S1. 2-vinylthiophene (10 mmol), azobisisobutyronitrile (0.03 mmol), and ethyl acetate (30 mmol) were mixed, heated and stirred at 70° C. for 2 hours to obtain poly (2-vinylthiophene);

[0054] Step S2. 1 g of graphene oxide and 0.6 g of polyethylene glycol-hyperbranched polyester were dissolved in 30 g of ethyl acetate according to weight ratio, 0.6 g of isophorone diisocyanate and 0.3 g of dibutyltin dilaurate were added, and the mixture was heated and stirred at 70° C. for 3 hours to obtain a copolymer;

[0055] Step S3. Add 0.6 g of isophorone diisocyanate and 0.3 g of poly(2-vinylthiophene) prepared in step S1 to the copolymer prepared in step S2, heat at 70°C for 4 hours, and after the reaction, soak the product in water, changing the water every 24 hours for 1 week, and then place it in a freeze dryer for freeze drying to obtain graphene oxide composite hydrogel.

[0056] Comparative Example 4: Preparation of graphene oxide composite hydrogel.

[0057] S1. 3-(2-thienyl)acrylic acid (10 mmol), azobisisobutyronitrile (0.03 mmol), and ethyl acetate (30 mmol) were mixed, heated and stirred at 70° C. for 2 hours to obtain poly(2-vinylthiophene);

[0058] Step S2. 1 g of graphene oxide and 0.6 g of polyethylene glycol-hyperbranched polyester were dissolved in 30 g of ethyl acetate according to weight ratio, 0.6 g of isophorone diisocyanate and 0.3 g of dibutyltin dilaurate were added, and the mixture was heated and stirred at 70° C. for 3 hours to obtain a copolymer;

[0059] Step S3. Add 0.6 g of isophorone diisocyanate and 0.3 g of poly(3-(2-thienyl)acrylic acid) obtained in step S1 to the copolymer obtained in step S2, heat at 70°C for 4 hours, and after the reaction, soak the product in water, changing the water every 24 hours for 1 week, and then place it in a freeze dryer for freeze drying to obtain graphene oxide composite hydrogel.

[0060] Comparative Example 5: Preparation of graphene oxide hydrogel.

[0061] The graphene oxide was soaked in water, the water was changed every 24 hours for one week, and then placed in a freeze dryer for freeze drying to obtain the graphene oxide hydrogel.

[0062] Performance Testing:

[0063] Adsorption performance: 0.1 g of the hydrogels prepared in Example 2 and Comparative Examples 1-5 were weighed, 40 mL of the metal ion solution was added, and the mixture was shaken for 12 hours. The concentration of the solution before and after adsorption was measured, and the adsorption amount was calculated.

[0064] Toughness: Take a hydrogel with a thickness of 5 mm as the sample material. The length and width of the sample material are not less than 200 mm respectively. After bending the sample material 90 degrees, record whether there are cracks and / or fractures at the bending point.

[0065] Tensile strength: The synthesized hydrogel was subjected to a tensile strength test using a CMT4102 universal testing machine at room temperature. The sample used for the tensile test had a diameter of 5 mm, a length of 30 mm, and a tensile rate of 50 mm / min.

[0066] Compressive strength: The compressive strength of the synthesized hydrogel was tested using a CMT4102 universal testing machine at room temperature, and the load when the compression deformation of the hydrogel sample was 10% was recorded.

[0067] Fatigue resistance: The fatigue resistance test was conducted on an electronic universal testing machine (UTM6104). A certain tensile strain was set, and the hydrogel sample was subjected to multiple non-intermittent load-unloading tensile tests at a tensile rate of 100 mm / min to obtain the corresponding stress-strain curve. Under the premise that the mechanical properties (strength, dissipated energy, etc.) of the hydrogel (dissipated energy refers to the area of ​​the ring enclosed by the stress-strain curve and the horizontal axis during the load-unloading tensile test of the hydrogel, and the area of ​​the ring represents the energy dissipated per unit volume of the hydrogel) remain stable after multiple cycles, the number of cycles that the hydrogel can withstand is the fatigue resistance of the hydrogel.

[0068] Table 1. Performance test results of graphene oxide composite hydrogels prepared in Example 2 and Comparative Examples 1-5.

[0069]

[0070] As can be seen from Table 1, the graphene oxide composite hydrogel prepared in Example 2 has good adsorption performance for heavy metals, high tensile strength, high compressive strength, good toughness and good fatigue resistance; the graphene oxide composite hydrogel prepared in Comparative Example 1 does not contain hyperbranched polyester, and the mechanical properties of the prepared graphene oxide composite hydrogel are slightly reduced; Comparative Example 2 does not contain polyethylene glycol, and the mechanical properties of the prepared graphene oxide composite hydrogel are slightly reduced; the polythiophene in Comparative Example 3 does not contain a carboxyl group, and cannot react with the carboxyl and hydroxyl groups on the graphene oxide molecular structure, the hyperbranched polyester containing polyethylene glycol, and the polythiophene in ... The carboxyl and hydroxyl groups on the molecular structure of the copolymer react with diisocyanate to form a cross-linked structure, and the mechanical properties of the obtained graphene oxide composite hydrogel are reduced. In addition, there is no carbonyl group in polythiophene, and π-π conjugation cannot be formed between molecules, so the adsorption performance of the graphene oxide composite hydrogel for heavy metals is reduced; in comparative example 4, there is no carbonyl group in the polythiophene, and π-π conjugation cannot be formed between molecules, so the adsorption performance of the graphene oxide composite hydrogel for heavy metals is reduced; comparative example 5 uses pure graphene oxide hydrogel, and the adsorption and mechanical properties of pure graphene oxide hydrogel for heavy metals are weak.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that after reading the specification of this application, the technicians can still modify or replace the specific implementation mode of the present invention with equivalents, but these modifications or changes do not deviate from the scope of protection of the pending claims of the present application.

Claims

1. A graphene oxide composite hydrogel, characterized in that: The graphene oxide composite hydrogel is polymerized by graphene oxide, a hyperbranched polyester copolymer containing polyethylene glycol, and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) in a weight ratio of 1:0.5-0.8:0.2-0.5; The method for preparing graphene oxide composite hydrogel comprises the following steps: Step S1. dissolving graphene oxide and a hyperbranched polyester copolymer containing polyethylene glycol in a second solvent according to a weight ratio, adding diisocyanate and a catalyst, heating and stirring, and obtaining a copolymer. Step S2. Add diisocyanate and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) to the copolymer obtained in step S1, heat to react, soak the product in deionized water, and freeze-dry to obtain a graphene oxide composite hydrogel.

2. The graphene oxide composite hydrogel according to claim 1, characterized in that The graphene oxide composite hydrogel is prepared by polymerizing graphene oxide, a hyperbranched polyester copolymer containing polyethylene glycol, and poly(trans-4-carbonyl-4-(thiophene-2-yl)but-2-enoic acid) in a weight ratio of 1:0.6:0.

3.

3. The graphene oxide composite hydrogel according to claim 2, characterized in that The hyperbranched polyester copolymer containing polyethylene glycol is selected from at least one of polyethylene glycol-hyperbranched polyester, polylactic acid-co-glycolic acid-polyethylene glycol-hyperbranched polyester, polylactic acid-polyethylene glycol-hyperbranched polyester, and polycaprolactone-polyethylene glycol-hyperbranched polyester.

4. The graphene oxide composite hydrogel according to any one of claims 1 to 2, characterized in that: The preparation method of the poly(trans-4-carbonyl-4-(thiophene-2-yl)but-2-enoic acid) comprises the following steps: Trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid, an initiator and a first solvent are mixed, heated and stirred for 1-3 hours to obtain poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid).

5. The graphene oxide composite hydrogel according to claim 4, characterized in that The initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile and lauroyl peroxide.

6. The graphene oxide composite hydrogel according to claim 4, characterized in that The molar ratio of the initiator to trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid is 0.001 to 0.004:

1.

7. A method for preparing the graphene oxide composite hydrogel according to claim 1, characterized in that: The steps include: Step S1. dissolving graphene oxide and a hyperbranched polyester copolymer containing polyethylene glycol in a second solvent according to a weight ratio, adding diisocyanate and a catalyst, heating and stirring, to obtain a copolymer; Step S2. Add diisocyanate and poly(trans-4-carbonyl-4-(thiophen-2-yl)but-2-enoic acid) to the copolymer obtained in step S1, heat to react, soak the product in deionized water, and freeze-dry to obtain a graphene oxide composite hydrogel.

8. The method for preparing graphene oxide composite hydrogel according to claim 7, wherein: In step S1, the catalyst is selected from at least one of stannous octoate and dibutyltin dilaurate.

9. The method for preparing graphene oxide composite hydrogel according to claim 7, wherein: The diisocyanate is at least one selected from the group consisting of xylene diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, p-xylylene diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.

10. Use of the graphene oxide composite hydrogel according to any one of claims 1 to 3 in the adsorption of heavy metals.