Alkali metal ion-modified carbon nitride, preparation method thereof, and application in photocatalytic H2O2 production
By using alkali metal ion-modified carbon nitride for photocatalytic production of H2O2 after hydrothermal and calcination treatments, the high cost and environmental pollution problems of H2O2 production in the existing technology are solved, and high efficiency in different water sources is achieved. , stable output and safety.
Patent Information
- Application Number
- CN202211329860.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-10-27
AI Technical Summary
Existing technologies have problems such as high cost, environmental pollution and explosion risks when producing hydrogen peroxide (H2O2), and the application of carbon nitride as a photocatalyst in actual water source environments has not been fully studied.
Using carbon nitride modified based on alkali metal ions, modified carbon nitride is prepared by adding alkali metal salts to dicyandiamine or melamine for hydrothermal reaction, followed by calcination and cleaning, and in river water, lake water or tap water systems Perform photocatalysis to produce H2O2.
The activity and stability of photocatalytic production of H2O2 are significantly improved. The activity of cesium ion-modified carbon nitride is increased by 21 times, and high-efficiency production is maintained in different water sources without attenuation. The amount of oxygen chemical adsorption is also greatly increased.
Smart Images

Figure CN115779944B_ABST
Abstract
Description
Technical field:
[0001] The present invention relates to the technical field of photocatalytic carbon nitride production of H2O2, and in particular to a carbon nitride modified by alkali metal ions, a preparation method thereof, and an application thereof in photocatalytic H2O2 production. Background technology:
[0002] Hydrogen peroxide, also known as hydrogen peroxide (chemical formula H2O2), is an important inorganic chemical product widely used in pulp bleaching, organic synthesis, environmental remediation, disinfection, fuel cells, and military applications. Furthermore, the use of H2O2 produces only water and reactive oxygen species, leaving it environmentally friendly and earning it the nickname "green product." Currently, the industry's most established H2O2 production methods rely on the anthraquinone process. This involves a multi-step hydrogenation and organic solvent oxidation process, followed by extraction and distillation. The reaction involves hydrogenation of 2-alkylanthraquinone to hydroquinone over a palladium catalyst, requiring large amounts of hydrogen and precious metal catalysts. This not only increases production costs but also poses environmental risks. Other methods utilize the direct combination of hydrogen and oxygen over precious metal catalysts; however, this reaction is prone to explosion, requiring the ratio of hydrogen and oxygen to remain below the explosive limit. Photocatalytic H2O2 production, however, is a safe and H2-free method that operates at room temperature. At the same time, carbon nitride (carbon nitride) as a photocatalyst has high selectivity in this reaction and has therefore been extensively studied.
[0003] Carbon nitride is a photocatalyst for producing H2O2. Common modification methods include preparing composite semiconductors, molecular doping, element doping, surface sensitization, etc. Among them, element doping is more commonly used, and the main doping elements are Na, K, P, etc. Although these modification methods have greatly increased the amount of photocatalytic H2O2 production, there has been no research on its performance in river water, lake water, and tap water systems. As we all know, H2O2 is the main reactant of Fenton's advanced oxidation technology, and Fenton's advanced oxidation technology is mainly used in fields such as sewage treatment. Therefore, it is very necessary to explore the photocatalytic H2O2 production technology of carbon nitride in actual water source environments (such as river water, lake water, tap water, etc.). Summary of the invention:
[0004] The present invention solves the problems existing in the prior art and provides a carbon nitride modified with alkali metal ions, a preparation method thereof, and an application in photocatalytic H2O2 production. The photocatalytic H2O2 production activity of the alkali metal ion-modified carbon nitride proposed in the present invention in river water, lake water, and tap water systems is not significantly attenuated compared to distilled water.
[0005] The object of the present invention is to provide a method for preparing carbon nitride based on alkali metal ion modification, comprising the following steps:
[0006] (1) adding an alkali metal salt to dicyandiamide or melamine, then adding water and stirring uniformly, performing a hydrothermal reaction, cooling after the hydrothermal reaction, and drying to obtain a white solid, wherein the alkali metal salt is a rubidium salt and / or a cesium salt;
[0007] (2) calcining the white solid obtained in step (1) and cooling it to room temperature to obtain a yellow solid, which is then washed and dried to obtain alkali metal ion-modified carbon nitride.
[0008] Preferably, the rubidium salt is rubidium chloride or cesium chloride, and the cesium salt is cesium chloride or cesium nitrate.
[0009] Preferably, the mass ratio of the dicyandiamide or melamine to the alkali metal salt in step (1) is 1:0.06-0.14, and the mass volume ratio of the alkali metal salt to water is 0.006-0.014:1 g / mL.
[0010] Preferably, the reaction temperature of the hydrothermal reaction in step (1) is 160° C.-200° C., and the reaction time is 8-12 h.
[0011] Preferably, the calcination temperature in step (2) is 500° C.-600° C., the calcination time is 2-4 h, and the heating rate is 2-10° C. / min.
[0012] Preferably, the yellow solid in step (2) is washed and dried to obtain modified carbon nitride in the following specific steps: the yellow solid is ground into powder, and filtered and washed with distilled water and ethanol respectively to obtain alkali metal ion-modified carbon nitride.
[0013] The present invention also protects the alkali metal ion-modified carbon nitride prepared by the above preparation method.
[0014] The present invention also protects the use of the above-mentioned alkali metal ion-modified carbon nitride in photocatalytic H2O2 production, comprising the following steps:
[0015] S1. Put the alkali metal ion-modified carbon nitride into a reaction vessel, add an ethanol aqueous solution, and stir to uniformly disperse the alkali metal ion-modified carbon nitride in the ethanol aqueous solution;
[0016] S2. Place the reaction container in step S1 in a multi-channel reactor (Perfil PCX-50C), introduce cooling circulating water at 10°C, stir, and continuously introduce oxygen while irradiating with LED white light or xenon lamp to obtain H2O2.
[0017] The alkali metal ion-modified carbon nitride proposed in the present invention is specifically used for photocatalytic production of H2O2 in river water, lake water or tap water systems.
[0018] Preferably, the mass volume ratio of the alkali metal ion-modified carbon nitride to the ethanol aqueous solution in step S1 is 0.0006-0.001:1 g / mL, and the volume fraction of the ethanol aqueous solution is 10%-15%.
[0019] Preferably, the illumination time in step S2 is 50-70 min.
[0020] Preferably, the oxygen flow rate is 1.3 mL / min and the power of the LED white light is 30.69 mW / cm 2 .
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] 1. The alkali metal ion-modified carbon nitride proposed in the present invention has good photocatalytic H2O2 production activity, especially the cesium ion-modified carbon nitride (CN-Cs) has a photocatalytic H2O2 production activity that is 21 times higher than that of unmodified carbon nitride.
[0023] 2. The photocatalytic H2O2 production activity of cesium ion modified carbon nitride (CN-Cs) in river water, lake water, and tap water systems did not show any significant attenuation compared to distilled water. The H2O2 production of cesium ion modified carbon nitride (CN-Cs) exceeded 8 mmol / g when continuously exposed to light for 12 hours, and there was no attenuation.
[0024] 3. The oxygen chemical adsorption capacity of cesium ion modified carbon nitride (CN-Cs) is 112.47 μmol / g, which is 8.53 times that of unmodified carbon nitride and is also better than the adsorption capacities of CN-K and CN-Rb (47.96 and 97.47 μmol / g, respectively). Description of the drawings:
[0025] Figure 1 1 is a Fourier transform infrared (FT-IR) spectrum of the cesium ion modified carbon nitride in Example 1 and the unmodified carbon nitride in Comparative Example 1.
[0026] Figure 2 1 is a structural diagram of the cesium ion-modified carbon nitride in Example 1 and the unmodified carbon nitride in Comparative Example 1.
[0027] Figure 3 These are pictures of water contact angles of the cesium ion-modified carbon nitride in Example 1, the unmodified carbon nitride in Comparative Example 1, the lithium ion-modified carbon nitride in Comparative Example 2, the sodium ion-modified carbon nitride in Comparative Example 3, the potassium ion-modified carbon nitride in Comparative Example 4, and the rubidium ion-modified carbon nitride in Comparative Example 5.
[0028] Figure 4It is the difference in dissolved oxygen (ΔDO) in the solution before and after the addition of the catalyst for the cesium ion-modified carbon nitride in Example 1, the unmodified carbon nitride in Comparative Example 1, the lithium ion-modified carbon nitride in Comparative Example 2, the sodium ion-modified carbon nitride in Comparative Example 3, the potassium ion-modified carbon nitride in Comparative Example 4, and the rubidium ion-modified carbon nitride in Comparative Example 5.
[0029] Figure 5 The H2O2 yields of the cesium ion modified carbon nitride in Example 4 and the unmodified carbon nitride in Comparative Example 1 under LED white light excitation.
[0030] Figure 6 The H2O2 yields of the cesium ion modified carbon nitride in Example 5 and the unmodified carbon nitride in Comparative Example 1 under visible light excitation.
[0031] Figure 7 The H2O2 yields of cesium ion-modified carbon nitride in different water source systems under LED white light excitation in Examples 4 and 6-8. Specific implementation method:
[0032] The following examples are provided to further illustrate the present invention, but are not intended to limit the present invention.
[0033] Unless otherwise defined, all technical terms used hereinafter have the same meanings as those generally understood by those skilled in the art. The technical terms used herein are for the purpose of describing specific embodiments only and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.
[0034] In the following examples, the oxygen flow rate is 1.3 mL / min and the power of the LED white light is 30.69 mW / cm 2 .
[0035] Example 1
[0036] The preparation method of carbon nitride modified by alkali metal ions comprises the following steps:
[0037] (1) Weigh 5 g of dicyandiamide and 0.5 g of cesium chloride and place them in a Teflon-lined hydrothermal autoclave. Add 50 mL of distilled water and stir on an electromagnetic stirrer at room temperature for 2 h.
[0038] (2) placing the hydrothermal reactor of step (1) in an oven at 180°C for hydrothermal reaction for 10 hours;
[0039] (3) After the hydrothermal reaction in step (2) is completed, the cooled reaction solution is dried in an oven at 80° C. for 10 h to obtain a white solid;
[0040] (4) calcining the white solid obtained in step (3) in a muffle furnace at 550° C. for 4 h at a heating rate of 4° C. / min, and cooling to room temperature to obtain a yellow solid;
[0041] (5) The yellow solid powder obtained in step (4) was ground and filtered and washed three times with distilled water and ethanol respectively, and finally dried to obtain cesium ion-modified carbon nitride, which was recorded as CN-Cs.
[0042] Comparative Example 1
[0043] The preparation of unmodified carbon nitride comprises the following steps:
[0044] (1) Weigh 5 g of dicyandiamide and calcine it in a muffle furnace at 550°C for 4 h at a heating rate of 2°C / min. After cooling to room temperature, a yellow solid was obtained.
[0045] (2) Grind the yellow solid powder obtained in step (2) to obtain unmodified carbon nitride, which is recorded as CN.
[0046] like Figure 1 and Figure 2 As shown, the structure of CN-Cs obtained in Example 1 is similar to that of CN obtained in Comparative Example 1. The structure of CN-Cs successfully introduces Cs + .
[0047] Comparative Example 2
[0048] The same as Example 1, except that cesium chloride is replaced by lithium chloride.
[0049] Comparative Example 3
[0050] The same as Example 1, except that cesium chloride is replaced by sodium chloride.
[0051] Comparative Example 4
[0052] The same as Example 1, except that cesium chloride is replaced by potassium chloride.
[0053] Comparative Example 5
[0054] The same as Example 1, except that cesium chloride is replaced by rubidium chloride.
[0055] like Figure 3 As shown in Figure 2, the water contact angle of CN-Cs is the smallest and its hydrophilicity is the best. Figure 4 As shown in the figure, CN-Cs has the highest dissolved oxygen difference, and it can autonomously adsorb a large amount of oxygen in the air.
[0056] Example 2
[0057] The preparation method of carbon nitride based on cesium ion modification includes the following steps:
[0058] (1) Weigh 5 g of melamine and 0.3 g of cesium chloride and place them in a Teflon-lined hydrothermal autoclave. Add 50 mL of distilled water and stir on an electromagnetic stirrer at room temperature for 2 h.
[0059] (2) placing the hydrothermal reactor of step (1) in an oven at 170°C for hydrothermal reaction for 11 hours;
[0060] (3) After the hydrothermal reaction in step (2) is completed, the cooled reaction solution is dried in an oven at 80° C. for 10 h to obtain a white solid;
[0061] (4) calcining the white solid obtained in step (3) in a muffle furnace at 500° C. for 4.5 h at a heating rate of 2° C. / min, and cooling to room temperature to obtain a yellow solid;
[0062] (5) The yellow solid powder obtained in step (4) was ground and filtered and washed three times with distilled water and ethanol respectively, and finally dried to obtain cesium ion-modified carbon nitride, which was recorded as CN-Cs.
[0063] Example 3
[0064] The preparation method of carbon nitride based on cesium ion modification includes the following steps:
[0065] (1) Weigh 5 g of dicyandiamide and 0.7 g of cesium chloride and place them in a Teflon-lined hydrothermal autoclave. Add 50 mL of distilled water and stir on an electromagnetic stirrer at room temperature for 2 h.
[0066] (2) placing the hydrothermal reactor of step (1) in an oven at 190°C for a hydrothermal reaction for 9 hours;
[0067] (3) After the hydrothermal reaction in step (2) is completed, the cooled reaction solution is dried in an oven at 80° C. for 10 h to obtain a white solid;
[0068] (4) calcining the white solid obtained in step (3) in a muffle furnace at 600° C. for 3.5 h at a heating rate of 10° C. / min, and cooling to room temperature to obtain a yellow solid;
[0069] (5) The yellow solid powder obtained in step (4) was ground and filtered and washed three times with distilled water and ethanol respectively, and finally dried to obtain cesium ion-modified carbon nitride, which was recorded as CN-Cs.
[0070] Example 4
[0071] The application of cesium ion modified carbon nitride specifically includes the following steps:
[0072] (1) 0.03 g of CN-Cs obtained in Example 1 was placed in a reaction flask, 50 mL of ethanol aqueous solution (volume fraction 10%) was added, and ultrasonication was performed for 20 min to disperse it thoroughly.
[0073] (2) The reaction bottle in step (1) was placed in a multi-channel reactor (Perfil PCX-50C), cooled circulating water at 10°C was introduced, stirred, and illuminated with LED white light for 1 hour.
[0074] (3) After illumination, 3 mL of the reaction solution was collected every 15 min, centrifuged (10,000 rpm, 5 min), and 1 mL of the supernatant was collected.
[0075] (4) Add 1 mL of the supernatant from step (3) to 1.25 mL of distilled water, 0.8 mL of phosphate buffer, 50 μL of peroxidase, and 50 μL of N,N-diethyl-p-phenylenediamine, shake well to develop color, and measure the liquid using a UV-visible spectrophotometer. Calculate the H2O2 concentration based on the absorbance.
[0076] like Figure 5 As shown, it shows that CN-Cs has excellent activity.
[0077] Example 5
[0078] The application of cesium ion modified carbon nitride specifically includes the following steps:
[0079] (1) 0.05 g of CN-Cs obtained in Example 1 was placed in a reaction flask, 200 mL of ethanol aqueous solution (volume fraction 10%) was added, and ultrasonication was performed for 20 min to disperse it thoroughly.
[0080] (2) Stir the reaction flask in step (1) and irradiate with xenon lamp light for 12 h (λ>420 nm).
[0081] (3) After illumination, 3 mL of the reaction solution was collected every 1 h, centrifuged (10,000 rpm, 5 min), and 1 mL of the supernatant was collected.
[0082] (4) Add 1 mL of the supernatant from step (3) to 1.25 mL of distilled water, 0.8 mL of phosphate buffer, 50 μL of peroxidase, and 50 μL of N,N-diethyl-p-phenylenediamine, shake well to develop color, and measure the liquid using a UV-visible spectrophotometer. Calculate the H2O2 concentration based on the absorbance.
[0083] like Figure 6 As shown, it shows that CN-Cs has excellent long-term stability.
[0084] Example 6
[0085] The application of cesium ion modified carbon nitride specifically includes the following steps:
[0086] (1) 0.03 g of CN-Cs obtained in Example 1 was placed in a reaction flask, 50 mL of 10% ethanol aqueous solution was added, and the mixture was thoroughly dispersed by ultrasonication for 20 min. The ethanol aqueous solution was prepared with river water.
[0087] (2) The reaction bottle in step (1) was placed in a multi-channel reactor (Perfil PCX-50C), cooled circulating water at 10°C was introduced, stirred, and illuminated with LED white light for 1 hour.
[0088] (3) After illumination, 3 mL of the reaction solution was collected every 15 min, centrifuged (10,000 rpm, 5 min), and 1 mL of the supernatant was collected.
[0089] (4) Add 1 mL of the supernatant from step (3) to 1.25 mL of distilled water, 0.8 mL of phosphate buffer, 50 μL of peroxidase, and 50 μL of N,N-diethyl-p-phenylenediamine, shake well to develop color, and measure the liquid using a UV-visible spectrophotometer. Calculate the H2O2 concentration based on the absorbance.
[0090] Example 7
[0091] The application of cesium ion modified carbon nitride specifically includes the following steps:
[0092] (1) Take 0.03g of CN-Cs obtained in Example 1 and place it in a reaction flask. Add 50mL of pure water and sonicate for 20min to disperse it thoroughly. The ethanol-water solution is prepared with lake water.
[0093] (2) The reaction bottle in step (1) was placed in a multi-channel reactor (Perfil PCX-50C), cooled circulating water at 10°C was introduced, stirred, and illuminated with LED white light for 1 hour.
[0094] (3) After illumination, 3 mL of the reaction solution was collected every 15 min, centrifuged (10,000 rpm, 5 min), and 1 mL of the supernatant was collected.
[0095] (4) Add 1 mL of the supernatant from step (3) to 1.25 mL of distilled water, 0.8 mL of phosphate buffer, 50 μL of peroxidase, and 50 μL of N,N-diethyl-p-phenylenediamine, shake well to develop color, and measure the liquid using a UV-visible spectrophotometer. Calculate the H2O2 concentration based on the absorbance.
[0096] Example 8
[0097] The application of cesium ion modified carbon nitride specifically includes the following steps:
[0098] (1) 0.03 g of CN-Cs obtained in Example 1 was placed in a reaction tube, 50 mL of ethanol aqueous solution (volume fraction 10%) was added, and ultrasonication was performed for 20 minutes to disperse the CN-Cs thoroughly. The ethanol aqueous solution was prepared with tap water.
[0099] (2) The reaction bottle in step (1) was placed in a multi-channel reactor (Perfil PCX-50C), cooled circulating water at 10°C was introduced, stirred, and illuminated with LED white light for 1 hour.
[0100] (3) After illumination, 3 mL of the reaction solution was collected every 1 h, centrifuged (10,000 rpm, 5 min), and 1 mL of the supernatant was collected.
[0101] (4) Add 1 mL of the supernatant from step (3) to 1.25 mL of distilled water, 0.8 mL of phosphate buffer, 50 μL of peroxidase, and 50 μL of N,N-diethyl-p-phenylenediamine, shake well to develop color, and measure the liquid using a UV-visible spectrophotometer. Calculate the H2O2 concentration based on the absorbance.
[0102] like Figure 7 As shown, it shows that CN-Cs has excellent activity in different systems.
[0103] Example 9
[0104] The application of cesium ion modified carbon nitride specifically includes the following steps:
[0105] (1) 0.03 g of CN-Cs obtained in Example 1 was placed in a reaction tube and purged under an inert atmosphere at 300° C. for 2 hours.
[0106] (2) After the temperature in step (1) drops to 50°C, continue to introduce 2000 ppm of O2 and adsorb for 2 hours until saturation.
[0107] (3) After the adsorption in step (2) is saturated, 50 mL / min Ar is introduced for 1 h. In an Ar atmosphere at 50 mL / min, the temperature is increased from 50°C to 500°C at a rate of 10°C / min. The released gas is detected by TCD.
[0108] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. Photocatalytic H production based on alkali metal ion-modified carbon nitride 2 O 2 Applications in It is characterized in that The steps include: S1. Place the alkali metal ion-modified carbon nitride in a reaction vessel, add an ethanol aqueous solution, and stir to uniformly disperse the alkali metal ion-modified carbon nitride in the ethanol aqueous solution, wherein the mass volume ratio of the alkali metal ion-modified carbon nitride to the ethanol aqueous solution is 0.0006-0.001:1 g / mL, and the volume fraction of the ethanol aqueous solution is 10%-15%; S2, placing the reaction container in step S1 in a multichannel reactor, stirring, continuously introducing oxygen, and irradiating with LED white light to obtain H 2 O 2 , the illumination time is 50-70min; The preparation method based on alkali metal ion modified carbon nitride comprises the following steps: (1) adding an alkali metal salt to dicyandiamide or melamine, then adding water and stirring evenly, performing a hydrothermal reaction, cooling after the hydrothermal reaction is completed, and drying to obtain a white solid, wherein the alkali metal salt is a cesium salt, the mass ratio of the dicyandiamide or melamine to the alkali metal salt is 1:0.06-0.14, the mass volume ratio of the alkali metal salt to water is 0.006-0.014:1 g / mL, the reaction temperature of the hydrothermal reaction is 160° C.-200° C., and the reaction time is 8-12 h; (2) calcining the white solid obtained in step (1) at a temperature of 500°C-600°C, a calcination time of 2-4h, and a heating rate of 2-10°C / min. After cooling to room temperature, a yellow solid is obtained. The yellow solid is washed and dried to obtain alkali metal ion-modified carbon nitride.
2. The use according to claim 1, It is characterized in that The cesium salt described in step (1) is cesium chloride or cesium nitrate.
3. The use according to claim 1, It is characterized in that The specific steps of washing and drying the yellow solid in step (2) to obtain modified carbon nitride are as follows: the yellow solid is ground into powder, and filtered and washed with distilled water and ethanol respectively to obtain alkali metal ion-modified carbon nitride.