A kind of organosilicon synergistic modified epoxy resin and its preparation method and use
By introducing silicone intermediates and phenolic substances into epoxy resins, an interpenetrating network structure is formed, which solves the problems of low heat resistance and low thermal residual weight of epoxy resins, and improves high temperature and mechanical properties, which are suitable for High temperature resistant materials in the aerospace and electronics fields.
Patent Information
- Application Number
- CN202211483117.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-24
AI Technical Summary
The application of existing epoxy resins in the aerospace field is limited by their low heat resistance and low thermal residual weight. Conventional methods to improve temperature resistance will lead to reduced processability and impact toughness, making it difficult to ensure both mechanical properties and high temperature performance.
By using silicone intermediates, epoxy resins, phenyl substances containing two unsaturated alkenyl groups, phenyl hydrogen-containing silicone oil and curing agents, etc., combined with catalysts and curing accelerators, we prepare excellent thermal stability and mechanics by combining them with a catalyst and a curing accelerator. The silicone modified epoxy resin with performance uses side chain modification and main chain expansion methods to form an interpenetrating network structure between silicone and epoxy resin.
It has achieved the high-temperature resistant materials in the aerospace and electronic electronics fields while maintaining the advantages of epoxy resin, and its thermal residual weight and mechanical properties are significantly improved, especially at 800°C. It is suitable for high-temperature resistant materials in the fields of aerospace and electronics.
Smart Images

Figure CN115785398B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of thermosetting resins, and in particular relates to an organosilicon-modified epoxy resin with improved heat resistance and thermal residual weight, and a preparation method and application thereof. Background Art
[0002] Ablative heat protection is a very effective and mature heat protection method developed in the 1950s. It is currently the most important heat protection technology for aircraft. Ablative heat protection materials are one of the most important parts of the thermal protection system and are widely used in the protection of internal structures and instruments of high-speed spacecraft. In thermal protection materials, whether it is a thermal protection coating or a resin-based composite material, the resin matrix is an important component of the thermal protection material. In ablative components, the resin plays an important role in providing and connecting carbon sources. The residual carbon and carbon layer structure of the resin are crucial to the ablation performance and thermal insulation performance. In addition, in the field of aerospace, advanced composite materials are used in main load-bearing components such as wings and fuselages due to their advantages such as light weight and high specific strength. Due to the effects of aerodynamics during high-speed flight, these materials are required to have excellent high temperature resistance and mechanical properties at the same time.
[0003] Epoxy resin is a widely used thermosetting resin. It has the advantages of excellent bonding strength, low curing shrinkage, good chemical stability, high mechanical strength, excellent electrical insulation and good processing performance. It is used as a matrix resin in adhesives, coatings and fiber-reinforced composites. However, epoxy resin itself has problems such as poor toughness and impact strength, poor thermal stability and low high-temperature thermal residual weight, which limits its application in the aerospace field. Conventional methods to improve the heat resistance of epoxy resin, such as introducing a rigid matrix and increasing the cross-linking density, will lead to poor processing and impact toughness. Silicone itself has the advantages of good flexibility, heat resistance and high thermal residual weight. Using silicone as an epoxy resin modifier can improve the flexibility and heat resistance of the resin while maintaining the advantages of epoxy resin, expanding the application scenarios of epoxy resin, such as epoxy resin ablation heat-resistant coatings under high-speed airflow scouring and high-residual carbon epoxy resin-based carbon fiber composites with integrated ablation structure.
[0004] The research work on silicone-modified epoxy resin mainly starts from the design of epoxy molecular structure. Through side chain grafting, main chain extension, cross-linking network design and other methods, high temperature resistant epoxy resin matrix with different temperature resistance grades is synthesized, aiming to improve the heat resistance and high temperature carbon residue of epoxy, and at the same time improve the flexibility of resin. In terms of side chain grafting, the modification of epoxy resin is mainly aimed at the epoxy active functional group and its expansion to introduce silicone intermediates. The side active functional group of bisphenol A type epoxy resin is mainly hydroxyl group, which is usually used to dehydrate and condense with the terminal hydroxyl group or terminal alkoxy group of silicone intermediate to realize the grafting of silicone side chain on epoxy resin. The expansion of epoxy active functional group also utilizes the reactivity of side hydroxyl group to realize the change of side functional group type. It mainly uses different types of silane coupling agents to modify the structure of epoxy resin, so that other types of functional groups such as vinyl are introduced into its side chain, and then the long chain of silicone intermediate is introduced through condensation reaction. However, due to the large differences in the side hydroxyl content of different types of epoxy resins, the amount of silicone intermediates introduced by side chain is limited. At the same time, due to the influence of steric hindrance and reaction activity, the introduction of silicone has the problem of low grafting rate. Free silicone molecular chains may also have an adverse effect on micro-compatibility and macro-material properties.
[0005] Therefore, the method of modifying epoxy resin with silicone has developed to expand the epoxy main chain, by opening some epoxy groups to produce more reactive sites, which is conducive to the introduction of silicone. Since there are more epoxy groups in the resin than side hydroxyl groups and the reaction activity is also stronger, the efficiency of introducing silicone on its molecular chain is greatly improved. At present, the expansion of the epoxy main chain is mainly through the opening of epoxy rings initiated by amino and hydroxyl groups. Although it is beneficial to the compatibility of silicone and epoxy resin, the consumption of epoxy groups will undoubtedly reduce the crosslinking density of the resin, thereby leading to a decrease in mechanical properties.
[0006] In order to solve the problem of reduced crosslinking density of modified resins, silicone-epoxy resin interpenetrating networks have become an important way to solve the problem. However, most of the current structural interpenetrations between silicone networks and epoxy networks have phase separation or large phase sizes, which is a key issue to be studied. In addition, there are other ways to modify epoxy resins with silicone, such as physical blending, selection or preparation of silicon-containing curing agents, etc., but such methods are difficult to simultaneously ensure the mechanical properties of epoxy resins, improve their high temperature resistance and high temperature residual carbon. Therefore, the development of a silicone-modified epoxy resin with both excellent thermal stability and mechanical properties requires one or more chain structure modification methods, and it is of great significance to achieve the synergistic modification of epoxy resins with multiple silicones. Summary of the invention
[0007] One of the purposes of the present invention is to provide a silicone-modified epoxy resin having excellent thermal stability and mechanical properties, and a preparation method and use thereof.
[0008] The invention provides an organosilicon-modified epoxy resin, which is prepared from materials including an organosilicon intermediate, an epoxy resin, a phenolic substance containing two unsaturated olefinic groups, a phenyl hydrogen-containing silicone oil and a curing agent as raw materials, wherein the mass ratio of the epoxy resin, the organosilicon intermediate, the phenolic substance containing two unsaturated olefinic groups and the phenyl hydrogen-containing silicone oil is 100:(1-100):(2-20):(1-50).
[0009] Furthermore, the mass ratio of the epoxy resin, the organosilicon intermediate, the phenolic substance containing two unsaturated olefinic groups, and the phenyl hydrogenated silicone oil is 100:(1-100):(2-20):(10-30).
[0010] Furthermore, the mass ratio of the epoxy resin, the organosilicon intermediate, the phenolic substance containing two unsaturated olefinic groups, and the phenyl hydrogenated silicone oil is 100:(10-30):(5-15):(15-25).
[0011] Furthermore, the mass ratio of the epoxy resin, the organosilicon intermediate, the phenolic substance containing two unsaturated olefinic groups, and the phenyl hydrogen-containing silicone oil is 100:(10-30):11:21.
[0012] Furthermore, the organosilicon intermediate is alkoxy-terminated methylphenyl polysiloxane, the epoxy resin is bisphenol A type epoxy resin, the phenolic substance containing two unsaturated alkenyl groups is diallyl bisphenol A, the phenyl hydrogen-containing silicone oil is hydrogen-terminated phenyl polysiloxane, and the curing agent is a diamine curing agent.
[0013] The raw materials also include an organic tin catalyst, a platinum catalyst and a curing accelerator.
[0014] Furthermore, the alkoxy-terminated methylphenyl polysiloxane is R is an alkyl group, a is the number of repeating units, and the molecular weight is 500 to 3000, preferably 1200;
[0015] The hydrogen-terminated phenyl polysiloxane is n1 and n2 are the number of repeating units, and the molecular weight is 500 to 3000, preferably 1000;
[0016] The bisphenol A epoxy resin is E51;
[0017] The organotin catalyst is dibutyltin dilaurate or stannous octoate;
[0018] The diamine curing agent is 4,4'-diamino-3,3'-dichlorodiphenylmethane or diaminodiphenylmethane;
[0019] The curing accelerator is N,N-benzyldimethylamine.
[0020] Further, the mass ratio of the epoxy resin to the organotin catalyst is 100:(0.01-5.00);
[0021] And / or, the mass volume ratio of the epoxy resin to the platinum catalyst is 100:(10-70) g / uL;
[0022] And / or, the mass volume ratio of the epoxy resin to the curing accelerator is 100: (100-500) g / uL.
[0023] Further, the mass ratio of the epoxy resin to the organotin catalyst is 100:(0.05-0.15);
[0024] And / or, the mass volume ratio of the epoxy resin to the platinum catalyst is 100:40 g / uL;
[0025] And / or, the mass volume ratio of the epoxy resin to the curing accelerator is 100:150 g / uL.
[0026] The present invention also provides a method for preparing the above-mentioned organosilicon-modified epoxy resin, the method comprising the following steps:
[0027] (1) adding an organosilicon intermediate and an epoxy resin into a reaction device to react and obtain an intermediate product 1;
[0028] (2) adding a phenolic substance containing two unsaturated olefinic groups and phenyl hydrogen-containing silicone oil to the intermediate product 1, mixing them evenly, and reacting to obtain the intermediate product 2;
[0029] (3) Add a curing agent to the intermediate product 2, mix well, and cure to obtain a silicone-modified epoxy resin.
[0030] Furthermore, in step (1), an organic tin catalyst is also added to the reaction device;
[0031] In step (2), a platinum catalyst is also added to the intermediate product 1;
[0032] In step (3), a curing accelerator is also added to the intermediate product 2.
[0033] Furthermore, in step (1), the reaction temperature is 120-160° C., the reaction time is 3-7 hours, and the reaction is carried out under an inert gas atmosphere;
[0034] In step (2), the reaction temperature is 50-90° C., the reaction time is 0.5-3 h, and the reaction is carried out under an inert gas atmosphere;
[0035] In step (3), the curing conditions are: first curing at 130-170° C. for 1-3 hours, and then curing at 170-200° C. for 2-5 hours.
[0036] Furthermore, in step (1), the reaction temperature is 140° C., the reaction time is 5 h, and the reaction is carried out under an inert gas atmosphere;
[0037] In step (2), the reaction temperature is 70° C., the reaction time is 1 h, and the reaction is carried out under an inert gas atmosphere;
[0038] In step (3), the curing conditions are: first curing at 150° C. for 2 h, and then curing at 180° C. for 3 h.
[0039] The present invention also provides the use of the above-mentioned organosilicon-modified epoxy resin in preparing materials in the aerospace field, materials in the electronic and electrical field, ablation-resistant composite materials, etc.
[0040] Furthermore, the ablation-resistant composite material is a composite material obtained by taking the above-mentioned organosilicon-modified epoxy resin as a matrix and adding fillers.
[0041] The organosilicon-modified epoxy resin provided by the present invention has good compatibility, and the thermal residual weight at 800°C is increased by more than 40% while the tensile strength remains equivalent to that of E51, and it has excellent mechanical properties and thermal stability. The organosilicon-modified epoxy resin of the present invention can be used to prepare high-temperature resistant adhesives, high-temperature resistant coatings, high-temperature resistant structural parts, electrical seals and other products, and has broad application prospects in the fields of aerospace, electronics and electrical appliances.
[0042] The organosilicon-modified epoxy resin of the invention has readily available raw materials, a simple preparation method, controllable synthesis conditions and is suitable for industrial production.
[0043] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0044] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 : EUD30-30 sample (c, f), control sample 1-1 (a, d), control sample 1-2 (b, e); ×1000: a, b, c, ×5000: d, e, f.
[0046] Figure 2 : Dynamic mechanical properties characterization results.
[0047] Figure 3 : Tensile strength and elongation at break test results.
[0048] Figure 4 : TGA test results. DETAILED DESCRIPTION
[0049] The raw materials and equipment used in the present invention are all known products, which are obtained by purchasing commercially available products.
[0050] Organic silicon intermediate PMPS-S is organic silicon intermediate IC232, with a molecular weight of 1200 and a structural formula of
[0051] The molecular weight of phenyl hydrogen silicone oil UC-233 is 1000, and the structural formula is
[0052] Example 1: Preparation of silicone-modified epoxy resin
[0053] 1. Preparation of methoxy-terminated organosilicon-grafted epoxy resin
[0054] Add the organosilicon intermediate IC232 and epoxy resin E51 into a three-necked flask according to the ratio in Table 1, raise the temperature to 140°C and introduce nitrogen to exhaust the air, stir evenly, then add the catalyst dibutyltin dilaurate (DBTDL for short), react for 5 hours to obtain the end-methoxy organosilicon grafted modified epoxy resin, and cool to room temperature for the next experimental operation.
[0055] 2. Modification of phenyl hydrogen silicone oil by diallyl bisphenol A
[0056] Add diallyl bisphenol A (DABPA for short) and phenyl hydrogen silicone oil UC233 into the three-necked flask in step 1 according to the ratio in Table 1, raise the temperature to 75°C and introduce nitrogen to exhaust the air, stir evenly, then add 40uL of platinum catalyst, react for 1h, and obtain an intermediate with a certain organosilicon cross-linking network.
[0057] 3. Prepare epoxy resin prepolymer and cure it
[0058] The intermediate obtained in step 2 and the melted curing agent 4,4'-diamino-3,3'-dichlorodiphenylmethane (MOCA) were mixed according to the proportions in Table 1 and stirred evenly. Then, 150 μL of N,N-benzyldimethylamine (BDMA) was added to the reaction device. The temperature was raised to 120° C. while nitrogen was introduced to exhaust the air. The mixture was stirred evenly and reacted for 1 hour to obtain an epoxy resin prepolymer.
[0059] The epoxy resin prepolymer is vacuum-debubbled, then poured into a preheated polytetrafluoroethylene mold, and placed in an oven for curing to obtain EUDS series silicone-modified epoxy resins: EUD30-10, EUD30-20, and EUD30-30.
[0060] The curing conditions are first at 150°C for 2 hours and then at 180°C for 3 hours.
[0061] Table 1. EUDS series silicone modified epoxy resin feed ratio
[0062] Sample name E51 / g DABPA / g UC233 / g IC232 / g DBTDL / g MOCA / g EUD30-10 100 11 21 10 0.05 40 EUD30-20 100 11 21 20 0.1 40 EUD30-30 100 11 21 30 0.15 40
[0063] The following is the preparation method of the control sample.
[0064] Comparative Example 1: Preparation of ES system materials
[0065] Add the organosilicon intermediate PMPS-S and epoxy resin E51 into a three-necked flask according to the ratio in Table 2, raise the temperature to 140°C and introduce nitrogen to exhaust the air, stir evenly, then add the catalyst DBTDL, react for 5 hours, cool to room temperature, and obtain ES system materials: ES10, ES20, ES30, ES50.
[0066] Table 2. Ratio of materials in ES system
[0067] Sample name E51 / g PMPS-S / g DBTDL / g ES10 100 10 0.05 ES20 100 20 0.1 ES30 100 30 0.15 ES50 100 50 0.25
[0068] Comparative Example 2: Preparation of EUD System Materials
[0069] 1. Modification of phenyl hydrogen silicone oil by diallyl bisphenol A
[0070] According to the ratio in Table 3, epoxy resin E51, diallyl bisphenol A and phenyl hydrogen silicone oil UC-233 were added to a three-necked flask, the temperature was raised to 75°C and nitrogen was introduced to exhaust the air, the mixture was stirred evenly, and then 40uL of platinum catalyst was added and reacted for 1h to obtain an intermediate with a certain organosilicon cross-linking network.
[0071] 2. Prepare epoxy resin prepolymer and cure it
[0072] The intermediate obtained in step 1 and the molten curing agent MOCA were mixed according to the proportions in Table 3, stirred evenly, and then 150 μL of BDMA was added to the reaction device. The temperature was raised to 120° C. while nitrogen was introduced to exhaust the air. The mixture was stirred evenly and reacted for 1 hour to obtain an epoxy resin prepolymer.
[0073] The epoxy resin prepolymer is vacuum-debubbled, then poured into a preheated polytetrafluoroethylene mold, and placed in an oven for curing to obtain EUD series silicone-modified epoxy resin materials: EUD10, EUD30, and EUD30.
[0074] The curing conditions are first at 150°C for 2 hours and then at 180°C for 3 hours.
[0075] Table 3. EUD system material ratio
[0076] Sample name E51 / g DABPA / g UC233 / g MOCA / g EUD10 100 4.4 8.8 40 EUD30 100 11 21 40 EUD50 100 17.6 35.2 40
[0077] Comparative Example 3: Preparation of comparative EUDS series materials
[0078] According to the ratio shown in Table 4 and referring to the method of Example 1, control EUDS series materials were prepared: EUD30-40, EUD30-50, and EUD30-70.
[0079] Table 4. EUDS series control material feed ratio
[0080] Sample name E51 / g DABPA / g UC233 / g IC232 / g DBTDL / g MOCA / g EUD30-40 100 11 21 40 0.20 40 EUD30-50 100 11 21 50 0.25 40 EUD30-70 100 11 21 70 0.35 40
[0081] Experiments have shown that in the process of preparing EUD30-40, EUD30-50 and EUD30-70, the first step produces small molecule alcohol substances as side reactions. As the subsequent curing reaction proceeds, the viscosity of the prepolymer increases, but at the same time, the curing temperature rises to the boiling point of the small molecule alcohol substances and overflows, resulting in void defects in the normal pressure curing casting. The presence of these void defects leads to the poor mechanical properties of EUD30-40, EUD30-50 and EUD30-70.
[0082] Comparative Example 4: Preparation of Cured Epoxy Resin E51
[0083] E51 and the molten curing agent (abbreviated as MOCA) were mixed according to the proportions in Table 5 and stirred evenly. Then 150 μL of BDMA was added to the reaction device. The temperature was raised to 120°C and nitrogen was introduced to exhaust the air. The mixture was stirred evenly and reacted for 1 hour to obtain an epoxy resin prepolymer.
[0084] The epoxy resin prepolymer was vacuum-debubbled, then poured into a preheated polytetrafluoroethylene mold, and placed in an oven for curing to obtain a cured epoxy resin E51.
[0085] The curing conditions are first at 150°C for 2 hours and then at 180°C for 3 hours.
[0086] Table 5. Feed ratio of curing epoxy resin E51
[0087] Sample name E51 / g MOCA / g Cured epoxy resin E51 100 40
[0088] The beneficial effects of the present invention are demonstrated by experimental examples below.
[0089] Experimental Example 1: Morphology Characterization
[0090] Test sample: EUD30-30 sample prepared in Example 1 (results see Figure 1 c, 1f); the system obtained by directly blending the organosilicon intermediate IC232 and the epoxy resin E51 in step 1 of Example 1 was used as the control sample 1-1 (the results are shown in Figure 1 a, 1d); the epoxy resin modified by grafting of methoxy-terminated organosilicon obtained in step 1 of Example 1 was used as control sample 1-2 (results see Figure 1 b, 1e).
[0091] Test method: The solidified sample was placed in liquid nitrogen for brittle fracture, and tested using a scanning electron microscope model JEOL JSM5900LV from JEOL Ltd. In order to ensure the conductivity of the sample surface, the cross section was vacuum sprayed with gold, the acceleration voltage was 5.0 kV, and then the brittle fracture surface of the sample was observed to explore the microscopic morphology.
[0092] Test results: Test results are as follows Figure 1 As shown. It can be seen that the compatibility of the EUDS series silicone-modified epoxy resin materials prepared in the embodiments of the present invention is significantly improved. From the experimental results, it can be seen that in the control sample 1-1, there is an obvious incompatibility between silicone and epoxy resin. After the grafting reaction, the silicone molecular chain and the epoxy network are connected together, and the island structure is an aggregate of silicone that has not been grafted. The addition of tertiary amines promotes the ring opening of the epoxy group and the grafting of the silicone molecular chain, and the overall compatibility is good. The scanning electron microscope photographs of these samples all have radial concentration points, and their textures are all in one direction, as if orientation has occurred. The unmodified E51 pure sample does not have such a phenomenon. The direction of the texture is related to the direction of the external stress, and the radial stress concentration points indicate that silicone plays a role in absorbing energy when the epoxy resin is subjected to stress.
[0093] Experimental Example 2: Dynamic Mechanical Properties (DMA) Characterization
[0094] Test samples: EUD30-10, EUD30-20 and EUD30-30 samples prepared in Example 1; the system obtained by directly blending the silicone intermediate IC232 and the epoxy resin E51 in Step 1 of Example 1 is used as the control sample 2-1 (named ES30-B); the epoxy resin modified by grafting of terminal methoxy silicone obtained in Step 1 of Example 1 is used as the control sample 2-2 (named ES30-G); EUD30 prepared in Control Example 2 is used as the control sample 2-3; and the cured epoxy resin E51 is used as the control sample 2-4.
[0095] Dynamic mechanical properties test method: TA Instruments' model Q800 dynamic mechanical analyzer was used. The sample size of the epoxy-cured sample was 20 mm × 10 mm × 4 mm. The three-point bending mode was used. The test frequency was 1 Hz, the amplitude was 20 um, the heating rate was 3 °C / min, and the temperature test range was 40 to 220 °C.
[0096] Test results: From Figure 2 It can be seen that the glass transition temperatures of ES30-B after direct blending and ES30-G after grafting with silicone are different, and ES30-B has a lower Tg. In addition, compared with control samples 2-1 to 2-4, the Tg of EUD30-10, EUD30-20 and EUD30-30 samples prepared in Example 1 of the present invention are lower, and EUD30-30 has the lowest Tg.
[0097] Experimental Example 3: Tensile Properties Test
[0098] Test samples: EUD30-10, EUD30-20 and EUD30-30 samples prepared in Example 1; EUD30 prepared in Control Example 2 as Control Sample 3-1; Cured epoxy resin E51 as Control Sample 3-2.
[0099] As mentioned above, the materials EUD30-40, EUD30-50, and EUD30-70 prepared in Control Example 2 have void defects, and the presence of these void defects leads to a decrease in the mechanical properties of EUD30-40, EUD30-50, and EUD30-70. Therefore, this experimental example did not test the tensile properties of EUD30-40, EUD30-50, and EUD30-70. Tensile performance test method: The tensile strength and elongation at break were tested using the UTM4204 electronic universal testing machine of Shenzhen Sansi Zongheng Technology Co., Ltd. The tensile properties of the samples were tested in accordance with the GB / T 528-2008 standard. The sample size was dumbbell-shaped, and the middle part of the sample was the test section, with a size of 80mm×10mm×4mm, and a tensile speed of 10mm / min.
[0100] Test results: The results are as follows Figure 3 As shown in the figure, it can be seen that the tensile strengths of EUD30-10, EUD30-20, and EUD30-30 are comparable to those of the cured epoxy resin E51, and the tensile strength of EUD30-10 is even slightly higher than that of the cured epoxy resin E51. In addition, the elongation at break of EUD30-10 is also higher than that of the cured epoxy resin E51.
[0101] Experimental Example 4: Thermal Stability Test
[0102] Test samples: EUD30-10, EUD30-20, EUD30-30, EUD30-40, EUD30-50, EUD30-70 samples; ES50 prepared in control example 1 is used as control sample 4-1; EUD30 prepared in control example 2 is used as control sample 4-2; cured epoxy resin E51 is used as control sample 4-3.
[0103] Thermogravimetric analysis (TGA) test method: The test was conducted using a TGA2 thermogravimetric analyzer from Mettler-Toledo, Switzerland. The test sample weight was 3-10 mg, the heating rate was 10°C / min, the test temperature range was 30-800°C, and the gas introduced was nitrogen.
[0104] Test results: The results are as follows Figure 4 As shown in Table 6, it can be seen that compared with the cured epoxy resin E51, the thermal stability of the EUDS series silicone modified epoxy resin material of the present invention is significantly improved. Among them, the thermal residual weight of EUD30-50 and EUD30-70 at 800°C is as high as more than 40%.
[0105] Table 6. Thermal stability test results under nitrogen atmosphere
[0106]
[0107]
[0108] In summary, the present invention provides a silicone-modified epoxy resin and a preparation method and use thereof. The present invention uses a silicone intermediate to graft an epoxy resin to obtain a side chain-modified epoxy resin, and further uses diallyl bisphenol A and phenyl hydrogen silicone oil to expand the epoxy main chain and construct a silicone cross-linking network, and finally solidifies to obtain a silicone-modified epoxy resin with good compatibility. The silicone-modified epoxy resin provided by the present invention has both excellent mechanical properties and thermal stability, and can be used to prepare high-temperature resistant adhesives, high-temperature resistant coatings, high-temperature resistant structural parts, electrical seals, and ablation-resistant composite materials and other products, and has broad application prospects in the fields of aerospace, electronics and electrical appliances.
Claims
1. Use of an organosilicon-modified epoxy resin in the preparation of aerospace materials, electronic and electrical materials, and ablation-resistant composite materials with high T5%, characterized in that: The organosilicon-modified epoxy resin is prepared from organosilicon intermediates, epoxy resins, phenolic substances containing two unsaturated alkenyl groups, phenyl hydrogen-containing silicone oil, curing agent, organotin catalyst, platinum catalyst and curing accelerator as raw materials, and the mass ratio of the epoxy resin, the organosilicon intermediate, the phenolic substances containing two unsaturated alkenyl groups and the phenyl hydrogen-containing silicone oil is 100:10:11:21; The organosilicon intermediate is alkoxy-terminated methylphenyl polysiloxane, the epoxy resin is bisphenol A type epoxy resin, the phenolic substance containing two unsaturated alkenyl groups is diallyl bisphenol A, the phenyl hydrogen-containing silicone oil is hydrogen-terminated phenyl polysiloxane, and the curing agent is a diamine curing agent; The alkoxy-terminated methylphenyl polysiloxane is R is an alkyl group, a is the number of repeating units, and the molecular weight is 500 to 3000; The hydrogen-terminated phenyl polysiloxane is n1 and n2 are the number of repeating units, and the molecular weight is 500 to 3000; The bisphenol A epoxy resin is E51; The organotin catalyst is dibutyltin dilaurate or stannous octoate; The diamine curing agent is 4,4'-diamino-3,3'-dichlorodiphenylmethane; The curing accelerator is N,N-benzyldimethylamine; The mass ratio of the epoxy resin to the organotin catalyst is 100:(0.01-5.00); The mass volume ratio of the epoxy resin to the platinum catalyst is 100:(10-70) g / uL; The mass volume ratio of the epoxy resin to the curing accelerator is 100: (100-500) g / uL; The preparation method of the organosilicon-modified epoxy resin comprises the following steps: (1) adding an organosilicon intermediate, an epoxy resin, and an organotin catalyst into a reaction device to react and obtain an intermediate product 1; (2) adding a phenolic substance containing two unsaturated olefinic groups, phenyl hydrogen-containing silicone oil, and a platinum catalyst to the intermediate product 1, mixing them evenly, and reacting to obtain an intermediate product 2; (3) Add a curing agent and a curing accelerator to the intermediate product 2, mix them evenly, and cure them to obtain a silicone-modified epoxy resin.
2. The use according to claim 1, characterized in that: The mass ratio of the epoxy resin to the organotin catalyst is 100:(0.05-0.15); And / or, the mass volume ratio of the epoxy resin to the platinum catalyst is 100:40 g / uL; And / or, the mass volume ratio of the epoxy resin to the curing accelerator is 100:150 g / uL.
3. The use according to claim 1, characterized in that: In step (1), the reaction temperature is 120-160° C., the reaction time is 3-7 h, and the reaction is carried out under an inert gas atmosphere; In step (2), the reaction temperature is 50-90° C., the reaction time is 0.5-3 h, and the reaction is carried out under an inert gas atmosphere; In step (3), the curing conditions are: first curing at 130-170° C. for 1-3 hours, and then curing at 170-200° C. for 2-5 hours.