Silicon carbide coated graphite susceptor and preparation method thereof

By combining the chemical vapor phase reaction method, high-pressure chemical vapor deposition method and low-pressure chemical vapor deposition method, the SiC coating is formed, which solves the problem of long preparation time, high cost and porousness of the silicon carbide coated graphite base, and improves the density and bonding strength. , suitable for industrial applications.

CN115786871BActive Publication Date: 2024-10-08ADVANCED FOR MATERIALS & EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211650737.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-10-08
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

In the prior art, the preparation of a silicon carbide-coated graphite base is time-consuming and costly, and the coating is porous and has weak bonding strength.

Method used

The chemical vapor reaction (CVR) method is used to form a SiC base layer on the surface of the graphite base, and then the high-pressure chemical vapor deposition method (HPCVD) is used to form an SiC intermediate layer on the SiC base layer. Finally, the low-pressure chemical vapor deposition method (LPCVD) is used to form an SiC intermediate layer on the SiC base layer. The SiC outer layer is formed on the SiC, and the three technologies are combined to improve the density and bonding strength, shorten the deposition time and reduce costs.

Benefits of technology

It achieves high density, low surface roughness and high bonding strength of the silicon carbide coated graphite base, shortens the deposition time to less than or equal to 10 hours, reduces production costs, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115786871B_ABST
    Figure CN115786871B_ABST
Patent Text Reader

Abstract

The present application discloses a silicon carbide coated graphite base and a preparation method thereof, wherein the preparation method comprises the following steps: firstly forming a SiC base layer on the surface of the graphite base by using a CVR technique, then forming a SiC intermediate layer on the SiC base layer by using a HPCVD technique, and finally forming a SiC outer layer on the SiC intermediate layer by using a LPCVD technique, wherein the SiC base layer is tightly bonded to the graphite base, and there is no obvious interface between the SiC intermediate layer and the SiC base layer, thereby effectively improving the density of the entire coating and the bonding strength between the coating and the graphite base, and the deposition speed of the SiC intermediate layer is accelerated under high pressure, thereby effectively reducing the production cost; when the coating thickness reaches 100 μm, only a total deposition time of less than or equal to 10 h is required, thereby saving production costs and being more conducive to industrialization; the SiC outer layer is smooth and dense, thereby effectively reducing the surface roughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of semiconductor graphite bases, and in particular to a silicon carbide coated graphite base and a preparation method thereof. Background Art

[0002] The third generation of semiconductor materials represented by gallium nitride (GaN) are widely used in solid-state light sources and power electronics, the "core" of microwave radio frequency devices, semiconductor lighting and other fields due to their superior properties such as large bandgap, high breakdown electric field, large thermal conductivity, high electron saturation drift rate, and strong radiation resistance. In particular, GaN materials have great application potential in the fields of semiconductor lighting (LED) and display because of their high efficiency, low loss and high frequency.

[0003] At present, GaN single crystal epitaxial growth technology is the most commonly used method for preparing single crystal GaN, among which silicon carbide (SiC) coated graphite susceptor is the key consumable in production, and the performance and quality of the susceptor play a vital role in the quality of the epitaxial layer of the wafer. Silicon carbide coated graphite susceptor has unique advantages: high purity, dense uniformity, and excellent thermal shock resistance and oxidation resistance, which improves product quality and process efficiency, thereby reducing overall operating costs. The preparation methods of silicon carbide coated graphite susceptor are currently widely used in chemical vapor deposition (Chemical Vapor Deposition, abbreviated as CVD) and chemical vapor reaction (Chemical Vapor Reaction, abbreviated as CVR). Among them, CVD mainly includes: low-pressure chemical vapor deposition (Low-pressure Chemical Vapor Deposition, abbreviated as LP CVD) and high-pressure chemical vapor deposition (High-pressure Chemical Vapor Deposition, abbreviated as HP CVD).

[0004] Although SiC coatings prepared by ordinary chemical vapor deposition and chemical reaction methods have high purity and good density, their deposition speed is slow. It takes 20 hours or more to deposit a coating with a thickness of 100 μm, and the production cost is very high. Summary of the invention

[0005] The invention provides a silicon carbide coated graphite susceptor and a preparation method thereof, so as to solve the technical problems of long time consumption and high cost in the preparation of the silicon carbide coated graphite susceptor in the prior art.

[0006] The technical solution provided by the present invention is as follows:

[0007] The first aspect of the present invention provides a method for preparing a silicon carbide coated graphite susceptor, comprising the following steps:

[0008] S1, placing the graphite base in a vacuum furnace after pretreatment; mixing Si powder and SiO2 powder and placing them in the vacuum furnace; evacuating the vacuum furnace and introducing argon gas to heat up to 1850°C to 2050°C, keeping the temperature, and forming a SiC base layer on the surface of the graphite base;

[0009] S2, lowering the temperature in the vacuum furnace to 1050° C. to 1200° C., setting the pressure to 1 KPa to 150 KPa, transporting trichloromethylsilane into the vacuum furnace through a carrier gas, introducing a dilution gas, and keeping the temperature to form a SiC intermediate layer on the SiC base layer;

[0010] S3. The pressure in the vacuum furnace is adjusted to 0.4 KPa to 1 KPa, trichloromethylsilane is transported into the vacuum furnace through a carrier gas, and a dilution gas is introduced to keep the temperature, so as to form a SiC outer layer on the SiC intermediate layer.

[0011] Furthermore, in the step S1, the molar ratio of the Si powder to the SiO2 powder is 1.05-1.10:1.

[0012] Furthermore, in the step S2, the formation time of the SiC intermediate layer is 2 hours.

[0013] Furthermore, in step S3, the formation time of the SiC outer layer is 4 hours.

[0014] Furthermore, in step S2 and step S3, the carrier gas is hydrogen, and the dilution gas is argon and hydrogen.

[0015] Furthermore, in step S2 and step S3, the flow rate of the carrier gas hydrogen is 2 L / min, the flow rate of the argon gas is 6 L / min, and the flow rate of the dilution hydrogen is 5 L / min.

[0016] Furthermore, in step S2 and step S3, the flow ratio of the carrier gas hydrogen to the trichloromethylsilane is 10:1.

[0017] Furthermore, the total thickness of the SiC base layer formed in the step S2 and the SiC intermediate layer formed in the step S1 is greater than or equal to 100 μm.

[0018] The second aspect of the present invention provides a silicon carbide coated graphite susceptor, which is prepared by the above-mentioned method for preparing the silicon carbide coated graphite susceptor.

[0019] Furthermore, the SiC intermediate layer is filled in the pores of the SiC base layer.

[0020] The preparation method of the silicon carbide coated graphite base of the present invention first uses CVR technology to form a SiC base on the surface of the graphite base, then uses HPCVD technology to form a SiC intermediate layer on the SiC base, and finally uses LPCVD technology to form a SiC outer layer on the SiC intermediate layer, wherein the SiC base is tightly combined with the graphite base, and there is no obvious interface between the SiC intermediate layer and the SiC base, which effectively improves the density of the entire coating and the bonding strength between the coating and the graphite base, and the deposition speed of the SiC intermediate layer is accelerated under high pressure, which effectively reduces the production cost; the SiC outer layer is smooth and dense, which effectively reduces the surface roughness. The preparation method of the silicon carbide coated graphite base combines HPCVD technology, LPCVD technology and CVR technology, ensures the performance of the SiC coating, and greatly shortens the deposition time of the coating. When the coating thickness reaches 100μm, only a total deposition time of less than or equal to 10h is required, which saves production costs and is more conducive to industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a flow chart of a method for preparing a silicon carbide coated graphite susceptor in an embodiment of the present invention;

[0023] Figure 2 This is a schematic diagram of the surface microscopic morphology of the coating on the silicon carbide coated graphite base prepared in Example 1 of the present invention;

[0024] Figure 3 Schematic diagram of coating thickness on the silicon carbide coated graphite base prepared in Example 1 of the present invention;

[0025] Figure 4 This is a schematic diagram of the cross-sectional microscopic morphology of the coating on the silicon carbide coated graphite base prepared in Example 1 of the present invention;

[0026] Figure 5 This is a microscope observation picture of the epitaxial growth of GaN single crystal on the silicon carbide coated graphite base prepared in Example 1 of the present invention;

[0027] Figure 6 This is a top view of a GaN single crystal epitaxially grown on a silicon carbide coated graphite susceptor prepared in Example 1 of the present invention after undergoing a high temperature furnace firing test;

[0028] Figure 7 This is a top view of the GaN single crystal epitaxially grown on the silicon carbide coated graphite base prepared in Example 1 of the present invention after being subjected to a high temperature furnace firing test. DETAILED DESCRIPTION

[0029] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0030] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the conditions under which this application can be implemented. Therefore, they have no substantive technical significance. Any structural modification, change in proportional relationship or adjustment of size should still fall within the scope of the technical content disclosed in this application without affecting the effects and purposes that can be achieved by this application.

[0031] like Figure 1 As shown, the embodiment of the present application provides a method for preparing a silicon carbide coated graphite base, comprising the following steps:

[0032] S1. Pre-treat the graphite base and place it in a vacuum furnace; mix Si powder and SiO2 powder and place them in a vacuum furnace; evacuate the vacuum furnace and introduce argon gas to heat it to 1850°C to 2050°C, keep it warm, and form a SiC base layer on the surface of the graphite base;

[0033] S2, lowering the temperature in the vacuum furnace to 1050° C. to 1200° C., setting the pressure to 1 KPa to 150 KPa, transporting trichloromethylsilane into the vacuum furnace through a carrier gas, introducing a dilution gas, and keeping the temperature to form a SiC intermediate layer on the SiC base layer;

[0034] S3. The pressure in the vacuum furnace is adjusted to 0.4 KPa to 1 KPa, trichloromethylsilane is transported into the vacuum furnace through a carrier gas, and a dilution gas is introduced to keep the temperature, so as to form a SiC outer layer on the SiC intermediate layer.

[0035] The chemical vapor reaction method (CVR) is to mix Si powder and SiO2 powder in a graphite crucible in a certain proportion, place a graphite base on the crucible, and react the SiO2 gas obtained at 1850℃~2050℃ in a high-temperature furnace with the graphite base to prepare a SiC coating. The SiC coating prepared by this method is tightly bonded to the substrate, and the coating thickness can reach more than 100μm, but the porosity of the material will still be retained.

[0036] Chemical vapor deposition (CVD) is mainly based on a certain deposition temperature, using trichloromethylsilane (CH3SiCl3, abbreviated as MTS) as a precursor, generally H2 as a diluent gas and carrier gas, Ar as a diluent gas, MTS is heated by oil temperature to present a gas form, and then brought into the deposition furnace by bubbling with carrier gas H2, and after a series of chemical reactions, a SiC coating is formed and deposited on the surface of the graphite base. The deposition temperature is 1050℃~1200℃, and the deposition pressure is 0.2KPa~150KPa. Among them, the study found that LPCVD technology is the most widely used, and the surface of the generated coating is smooth and dense; however, in the LPCVD process, due to the short residence time of the active products after the decomposition of the gas source in the furnace, the deposition rate of SiC on the substrate surface is low, and the raw material utilization rate is also low, resulting in a sharp increase in preparation costs, which seriously limits its industrialization process. In order to overcome the above problems, HPCVD is an effective way. Compared with LPCVD, HPCVD has a high deposition pressure, a long residence time of active substances after gas source decomposition, and a sufficient reaction, which can ultimately achieve rapid deposition of SiC. The SiC coating prepared by combining these two methods is high in purity, smooth and dense, and can quickly deposit a coating with a thickness of ≥100μm. However, the study found that the bonding strength of the generated SiC coating substrate is weak.

[0037] In the embodiment of the present application, the SiC base layer is first deposited on the graphite base by CVR technology, and the SiC base layer is tightly combined with the graphite base, which improves the bonding strength between the coating and the graphite base; then the SiC intermediate layer is formed on the SiC base layer by HPCVD technology, and it is found through characterization that there is no obvious interface between the SiC intermediate layer and the SiC base layer, indicating that the SiC intermediate layer fills the pores of the SiC base layer, effectively improving the density of the coating and the bonding strength between the coating and the graphite base; in addition, the combination of CVR technology and HPCVD technology can be deposited quickly, so that the thickness of the coating is greater than or equal to 100μm, and only needs to be deposited for less than 10h, which effectively reduces the cost. Finally, the SiC outer layer is formed on the SiC intermediate layer by LPCVD technology, and the SiC outer layer is smooth and dense, which effectively reduces the roughness of the coating surface. The SiC coating prepared on the surface of the graphite base in the embodiment of the present application has each coating tightly bonded, greatly improved overall performance, a smooth surface, and almost no defects such as pores and bubbles, thereby solving the technical problems of time-consuming and high-cost preparation of silicon carbide coated graphite bases, porous coatings, and weak interlayer bonding strength.

[0038] Furthermore, in step S1, the molar ratio of Si powder to SiO2 powder is 1.05 to 1.10: 1. In the actual process of preparing the coating, the amount of Si powder added is greater than the amount of SiO2, so that SiO2 can react completely.

[0039] According to a second aspect of the embodiments of the present application, a silicon carbide coated graphite base is provided, which is prepared by the above-mentioned preparation method.

[0040] The Si powder and SiO2 powder used in the following examples are high-purity Si powder and high-purity SiO2 powder, respectively, and the purity of both is above 99.99%.

[0041] Example 1

[0042] A method for preparing a silicon carbide coated graphite base, firstly, mixing high-purity Si powder and high-purity SiO2 powder, placing them at the bottom of a graphite crucible, and then placing the crucible in a vacuum furnace. To prevent residual SiO2 powder, the amount of Si powder is greater than that of SiO2 powder. In this embodiment, the mass of Si powder is 117g, and the mass of SiO2 powder is 251g. After pre-treatment, the graphite base is placed above a graphite gas diverter plate, the vacuum furnace is evacuated and heated in an argon atmosphere, and after heating to 1850°C at a rate of 10°C / min, the temperature is kept in the furnace for 2h to form a SiC base layer on the surface of the graphite base. Then the temperature in the vacuum furnace is lowered to 1100°C, the deposition pressure is set to 100KPa, trichloromethylsilane is transported to the vacuum furnace by carrier gas hydrogen, and argon and dilution hydrogen are introduced, the flow rate of carrier gas hydrogen is set to 2L / min, the flow rate of dilution hydrogen is set to 5L / min, the flow rate of argon is set to 6L / min, the insulation time is 2h, and a SiC intermediate layer is generated on the surface of the SiC base layer of the graphite base. Finally, the deposition pressure in the vacuum furnace is lowered to 500Pa, trichloromethylsilane is transported to the vacuum furnace by carrier gas hydrogen, and argon and dilution hydrogen are introduced, the flow rate of carrier gas hydrogen is 2L / min, the flow rate of dilution hydrogen is 5L / min, the flow rate of argon is 6L / min, the insulation time is 4h, and a SiC outer layer is formed on the SiC intermediate layer. The total deposition time of the three coatings in this embodiment is 8h.

[0043] The coating surface and cross section of the silicon carbide coated graphite base prepared in this embodiment were subjected to SEM analysis and detection. The analysis results are as follows: Figures 2 to 4 As shown, the dark part is the graphite base and the light part is the SiC coating. Figure 2 The surface of the SiC coating prepared in this embodiment is smooth and dense. Figure 3 , the thickness of the SiC coating prepared in this embodiment is greater than 100 μm. Figure 4 The SiC coating formed on the surface of the graphite base by the preparation method of this embodiment has a high purity and good density of the coating structure, there is no stratification between the SiC base layer, the SiC intermediate layer and the SiC outer layer, and the SiC coating is well bonded to the graphite base.

[0044] The performance of the SiC coating prepared in this example was tested. The SiC coated graphite pedestal is an important consumable for the epitaxial growth of GaN single crystals, so the growth of GaN single crystal wafers is an important indicator of the performance of the SiC coated graphite pedestal. Figure 5 The microscope characterization image of the GaN wafer is shown in the figure. It can be seen from the figure that a crack-free GaN film has been epitaxially grown on the SiC coated substrate. In addition, a high-temperature furnace test was conducted on the SiC coated graphite base. The test conditions were: temperature 1400°C, nitrogen and 5% hydrogen gas, and heat preservation for 3 hours. The following results were obtained: Figure 6 The top view of the object shown and Figure 7 The bottom view of the actual object shown in the figure shows that the coating has no cracks or peeling, indicating that the SiC coating has excellent thermal shock resistance.

[0045] Example 2

[0046] A method for preparing a silicon carbide coated graphite base, firstly, mixing high-purity Si powder and high-purity SiO2 powder, placing them at the bottom of a graphite crucible, and then placing the crucible in a vacuum furnace. To prevent residual SiO2 powder, the amount of Si powder is greater than that of SiO2 powder. In this embodiment, the mass of Si powder is 117g, and the mass of SiO2 powder is 251g. After pre-treatment, the graphite base is placed above a graphite gas diverter plate, the vacuum furnace is evacuated and heated in an argon atmosphere, and after heating to 1950°C at a rate of 15°C / min, the temperature is kept in the furnace for 2h to form a SiC base layer on the surface of the graphite base. Then the temperature in the vacuum furnace is lowered to 1150°C, the deposition pressure is set to 60KPa, trichloromethylsilane is transported to the vacuum furnace by carrier gas hydrogen, and argon and dilution hydrogen are introduced. The flow rate of carrier gas hydrogen is set to 2L / min, the flow rate of dilution hydrogen is set to 5L / min, and the flow rate of argon is set to 6L / min. The insulation time is 3h, and a SiC intermediate layer is generated on the surface of the SiC base layer of the graphite base. Finally, the deposition pressure in the vacuum furnace is lowered to 600Pa, trichloromethylsilane is transported to the vacuum furnace by carrier gas hydrogen, and argon and dilution hydrogen are introduced. The flow rate of carrier gas hydrogen is 2L / min, the flow rate of dilution hydrogen is 5L / min, and the flow rate of argon is 6L / min. The insulation time is 4h, and a SiC outer layer is formed on the SiC intermediate layer. The total deposition time of the three coatings in this embodiment is 9h.

[0047] Example 3

[0048] A method for preparing a silicon carbide coated graphite base, firstly, mixing high-purity Si powder and high-purity SiO2 powder, placing them at the bottom of a graphite crucible, and then placing the crucible in a vacuum furnace. To prevent residual SiO2 powder, the amount of Si powder is greater than that of SiO2 powder. In this embodiment, the mass of Si powder is 117g, and the mass of SiO2 powder is 251g. After pre-treatment, the graphite base is placed above a graphite gas diverter plate, the vacuum furnace is evacuated and heated in an argon atmosphere, and after heating to 2050°C at a rate of 12°C / min, the temperature is kept in the furnace for 2h to form a SiC base layer on the surface of the graphite base. Then the temperature in the vacuum furnace is reduced to 1200°C, the deposition pressure is set to 20KPa, trichloromethylsilane is transported to the vacuum furnace by carrier gas hydrogen, and argon and dilution hydrogen are introduced, the flow rate of carrier gas hydrogen is set to 2L / min, the flow rate of dilution hydrogen is set to 5L / min, the flow rate of argon is set to 6L / min, the insulation time is 4h, and a SiC intermediate layer is generated on the surface of the SiC base layer of the graphite base. Finally, the deposition pressure in the vacuum furnace is reduced to 800Pa, trichloromethylsilane is transported to the vacuum furnace by carrier gas hydrogen, and argon and dilution hydrogen are introduced, the flow rate of carrier gas hydrogen is 2L / min, the flow rate of dilution hydrogen is 5L / min, the flow rate of argon is 6L / min, the insulation time is 4h, and a SiC outer layer is formed on the SiC intermediate layer. The total deposition time of the three coatings in this embodiment is 10h.

[0049] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a silicon carbide coated graphite susceptor, characterized in that: The following steps are involved: S1, CVR deposition: pre-treat the graphite base and place it in a vacuum furnace; mix Si powder and SiO2 powder and place them in the vacuum furnace; evacuate the vacuum furnace and introduce argon protection to raise the temperature to 1850°C to 2050°C, keep the temperature, and form a SiC base layer on the surface of the graphite base; S2, HPCVD deposition: lowering the temperature in the vacuum furnace to 1050°C-1200°C, setting the pressure to 20KPa-100KPa, transporting trichloromethylsilane into the vacuum furnace through a carrier gas, introducing a dilution gas, and keeping the temperature to form a SiC intermediate layer on the SiC base layer; in the step S2, the formation time of the SiC intermediate layer is 2-4h; S3, LPCVD deposition: adjusting the pressure in the vacuum furnace to 0.5 KPa-0.8 KPa, transporting trichloromethylsilane into the vacuum furnace through a carrier gas, introducing a dilution gas, and keeping the temperature to form a SiC outer layer on the SiC intermediate layer; When the coating thickness reaches 100 μm, a total deposition time of less than or equal to 10 h is required; In step S2 and step S3, the carrier gas is hydrogen, and the dilution gas is argon and hydrogen; in step S2 and step S3, the flow rate of the carrier gas hydrogen is 2L / min, the flow rate of the argon gas is 6L / min, and the flow rate of the dilution hydrogen is 5L / min; in step S2 and step S3, the flow ratio of the carrier gas hydrogen to the trichloromethylsilane is 10:

1.

2. The method for preparing a silicon carbide coated graphite susceptor according to claim 1, characterized in that: In the step S1, the molar ratio of the Si powder to the SiO2 powder is 1.05-1.10:

1.

3. The method for preparing a silicon carbide coated graphite susceptor according to claim 1, characterized in that: In the step S3, the formation time of the SiC outer layer is 4 hours.

4. A silicon carbide coated graphite susceptor, characterized in that: The silicon carbide coated graphite susceptor is prepared by the preparation method of any one of claims 1 to 3.

5. The silicon carbide coated graphite susceptor according to claim 4, characterized in that: The SiC intermediate layer is filled in the pores of the SiC base layer.