A protective blue film for power battery and preparation method thereof

By optimizing the acrylic resin ratio and emulsion copolymerization method, an adhesive layer with high adhesion, cohesion and peel strength is prepared, which solves the problems of low peel force and poor cohesion of existing protective films for power batteries, and realizes the use of protective films for power batteries. The high temperature resistance and voltage breakdown performance of the protective film meet the needs of the battery block.

CN115820149BActive Publication Date: 2024-10-08GUANGDONG DONGLI NEW MATERIALS SCI & TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211237765.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-10
Publication Date
2024-10-08
Estimated Expiration
2042-10-10

AI Technical Summary

Technical Problem

Existing acrylic protective films for power batteries have low peeling force, poor cohesion, are prone to peeling, are not resistant to high temperatures and voltage breakdown, and cannot meet the needs of battery blocks.

Method used

By optimizing the ratio of a variety of acrylic resins containing polar groups, the emulsion copolymerization method is used to prepare the adhesive layer, combining methacrylate, butyl acrylate, modified acrylate monomers, silane coupling agents and isocyanate cross-linking The agent forms a methacrylate copolymer adhesive layer with a weight average molecular weight of 1 million to 1.5 million, which enhances the adhesion, cohesion and peel strength and ensures the warpage resistance, high temperature resistance and flame retardant properties of the blue film.

Benefits of technology

It achieves excellent adhesion, cohesion and peel strength of the protective blue film for power batteries, avoids edge warping, ensures battery performance, meets the high temperature and voltage requirements of the battery block, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the field of adhesive technology, in particular to the field of IPC C09J7, and more specifically to a protective blue film for a power battery and a preparation method thereof. The protective blue film for a power battery described in the present application is characterized in that the blue film comprises: a substrate layer, a glue layer and a release film layer. The preparation of the glue layer colloid is achieved by adjusting the weight ratio of the silane coupling agent and the isocyanate crosslinking agent to be 1-2:1-2. Since the silane coupling agent can form a Si-O-Si crosslinking network with a large bond energy between polymer molecular chains, the -NCO group in the isocyanate crosslinking agent and the -OH group in the glue layer can form a crosslinking network faster. Thereby, the thermal stability of the glue layer is improved, so that the glue layer achieves excellent adhesion and high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of adhesive technology, in particular to the field of IPCC09J7, and more specifically to a protective blue film for a power battery and a preparation method thereof. Background Art

[0002] New energy vehicles are developing at a very high speed and gradually occupying the market. Among them, power batteries are the core components of new energy vehicles and also the power source of electric vehicles. The requirements for their production capacity and quality are getting higher and higher. Coating blue film is an important process in the production process of power batteries. Blue film, also known as isolation film, anti-adhesion film, protective film, etc., has multiple colors such as red, green, blue, white, and black. It is divided into single-sided release film and double-sided release film. Blue film is usually used in power batteries. It is an insulating material. The blue film separates the battery cells from each other, blocking the impact of various faults on other battery cells caused by a single battery cell, and preventing the occurrence of "one loss and all losses". The blue film structure includes a substrate layer, a glue layer and a release film layer. The core is the glue layer, which is mainly divided into silicone type, rubber type and acrylic glue layer. The silicone type has a high synthesis cost and is not alkali-resistant, which is not conducive to the development of market popularity; the rubber type has a complex synthesis process and is not solvent-resistant, and lithium battery manufacturers rarely use it. Compared with the first two, acrylics have great advantages in cost, process and performance, and have superior overall performance. They are also the most widely used blue films.

[0003] CN201810576295.5 provides a UV-resistant protective film and a preparation method thereof, wherein the peeling force of the protective film changes within ±35% after high temperature and long-term UV irradiation by adjusting the component content, and there is no debonding, residual glue, or color difference after long-term UV irradiation. However, the peeling force of the protective film provided is relatively low.

[0004] CN202210333072.2 provides an acrylic ester adhesive, an adhesive tape and a preparation method thereof. The acrylic ester adhesive has a low biocarbon content and the tape has poor cohesion during use, which is prone to peeling. Summary of the invention

[0005] The present invention optimizes the ratio of various types of acrylic resins containing polar groups, and obtains a colloid with excellent adhesion, cohesion and peel strength through emulsion copolymerization. The specific adhesive layer gives the blue film good warping resistance and high temperature resistance, which can effectively ensure that the blue film does not warp during use, thereby effectively protecting the power battery. At the same time, the obtained protective blue film has excellent flame retardant properties and strong voltage breakdown resistance, and the blue film resistance can meet the use requirements of the battery block.

[0006] To achieve the above object, the present invention provides a protective blue film for a power battery, characterized in that the blue film comprises: a substrate layer, a glue layer and a release film layer:

[0007] The adhesive layer includes a first adhesive layer and a second adhesive layer;

[0008] The substrate layer includes a first substrate layer and a second substrate layer;

[0009] The structure of the blue film, from inside to outside, is the second substrate layer, the second adhesive layer, the first substrate layer, the first adhesive layer, and the release film layer;

[0010] The adhesive layer is a methacrylate copolymer with a weight average molecular weight of 1-1.5 million;

[0011] The release film layer material is selected from one of polypropylene, polyimide, and polyethylene terephthalate; the thickness of the substrate layer PET film is 20-30 μm;

[0012] Preferably, the substrate layer material is PET, purchased from Dongwan Zhonglian Electronic Materials Co., Ltd., with a thickness of 25 μm;

[0013] Preferably, the release film layer material is selected from polyethylene terephthalate, has a thickness of 25 μm, and is purchased from Suzhou Chenfan New Materials Co., Ltd.

[0014] The first adhesive layer and the second adhesive layer have the same composition;

[0015] The coating thickness of the adhesive layer is 25-30 μm;

[0016] The present invention provides a method for preparing a protective blue film colloid for a power battery.

[0017] The invention comprises the following raw materials in parts by weight: 35-40 parts of methyl methacrylate; 15-25 parts of butyl acrylate; 10-15 parts of modified acrylic ester monomer; 10-15 parts of tackifying resin; 1-4 parts of silane coupling agent; 1-4 parts of isocyanate crosslinking agent; 0.5-1 parts of initiator; 1-10 parts of dye; 1-2 parts of buffer; 1-2 parts of emulsifier; 1-2 parts of oxidant; 1-2 parts of reducing agent; 2-3 parts of pH regulator; 100 parts of deionized water;

[0018] Preferably, the emulsifier is sodium dodecylbenzene sulfonate (CAS No.: 25155-30-0);

[0019] Preferably, the buffer is 0.5 mol / L sodium bicarbonate solution (CAS No.: 144-55-8);

[0020] Preferably, the initiator is ammonium persulfate (CAS No.: 7727-54-0);

[0021] Preferably, the oxidant is tert-butyl hydroperoxide (CAS No.: 75-91-2);

[0022] Preferably, the reducing agent is sodium formaldehyde sulfoxylate (CAS No.: 870-72-4);

[0023] Preferably, the pH regulator is aqueous ammonia containing 27% ammonia;

[0024] Preferably, the dye is one or a mixture of indigo and phthalocyanine blue;

[0025] Further preferably, the dye is purchased from indigo dye produced by Yizhou Spinning Dyeing Company, model number CFX-1;

[0026] Preferably, the modified acrylic resin comprises: a hydroxyl monomer, a carboxyl monomer and an aromatic monomer;

[0027] Preferably, the hydroxy monomer includes: 4-hydroxybutyl methacrylate glycidyl ether or hydroxypropyl methacrylate or a mixture of the two;

[0028] More preferably, the hydroxy monomer is 4-hydroxybutyl methacrylate glycidyl ether (CAS No.: 119692-59-0)

[0029] Preferably, the carboxyl monomer is acrylic acid or crotonic acid or a mixture of the two;

[0030] Further preferably, the carboxyl monomer is acrylic acid (CAS No.: 79-10-7);

[0031] Preferably, the aromatic monomer comprises: phenyl methacrylate or aryl methacrylate or a mixture of the two;

[0032] Further preferably, the aromatic monomer is phenyl methacrylate (CAS No.: 2177-70-0);

[0033] Preferably, the alkane coupling agent includes: one or more of γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, and γ-aminopropyltrimethoxysilane;

[0034] Further preferably, the alkyl coupling agent is γ-aminopropyltrimethoxysilane (CAS No.: 13822-56-5)

[0035] Preferably, the isocyanate crosslinking agent includes: one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate;

[0036] Further preferably, the isocyanate crosslinking agent is isophorone diisocyanate (CAS No.: 4098-71-9);

[0037] Preferably, the tackifying resin is a terpene resin purchased from Jinlin Chemical, model number T100;

[0038] When the weight ratio of methyl methacrylate to terpene resin is 3-4:1, it can not only change the internal structure of the colloid, but also improve its surface properties, so that the polymer has excellent adhesion and obtains a technical effect that is conducive to processing. In the prior art, adding a small amount of tackifying resin can improve the cohesive energy of the polymer. In the tackifying resin / acrylate copolymer emulsion system, most of the tackifying resin is dispersedly attached to the periphery of the polyacrylate particles in the form of tiny particles. This shows that after the monomer solution of the tackifying resin is added to the seed emulsion and adsorbed to the surface of the seed emulsion during emulsion polymerization, the monomer molecules can gradually diffuse into the seed emulsion particles and perform polymerization there; the tackifying resin molecules are difficult to diffuse completely into the seed emulsion due to the relatively poor affinity with most acrylic ester polymers, and some are gradually precipitated on the surface of the seed emulsion particles. Due to this separation of the tackifying resin and the monomer, the monomer molecules entering the seed emulsion are reduced. When the amount of the tackifying resin is more, this phenomenon is more obvious, thereby reducing the cohesive force of the polymer. At the same time, after the tackifying resin exceeds a certain amount, it causes entanglement between molecular chains, affects the cohesive strength of the glue layer, thereby affects the adhesive properties of the glue layer, and reduces both the holding force and the initial adhesion. The present invention synthesizes an acrylic resin polymer with a number average molecular weight of 100,000-1.5 million, and the large molecular weight causes a smaller initial adhesion, while the methyl methacrylate selected by the present invention is close to the glass transition temperature of the terpene resin, and has good compatibility, so that the polymer colloid reaches excellent adhesion.

[0039] Preferably, the weight ratio of methyl methacrylate to terpene resin is 3-4:1.

[0040] A further preferred weight ratio of methyl methacrylate to terpene resin is 3:1;

[0041] When the weight ratio of methyl methacrylate to acrylic acid is 30:0.5-1, the colloid has both excellent adhesion and anti-warping properties. The reason is that the acrylic acid molecule carries a polar functional group carboxyl group. The active hydrogen atom in the carboxyl group can form a hydrogen bond with the ester group on the copolymer molecular segment, thereby enhancing the intermolecular force and improving the bonding performance. At the same time, the electronic effect of this polar group enhances the firmness of the adhesion between the copolymer and the surface of the polar adherend. With the addition of this ratio, the number of carboxyl groups introduced into the system and the cross-linking points and their distribution are just in an optimal state. When the amount of acrylic acid is too large, too many carboxyl groups are introduced into the polymer molecules, which will affect the normal polymerization of the emulsion, which is manifested as a significant decrease in the apparent viscosity of the emulsion, thereby producing gel defects and causing a decrease in adhesion.

[0042] Preferably, the weight ratio of methyl methacrylate to carboxyl monomer is 30:0.5-1;

[0043] Further preferably, the weight ratio of methyl methacrylate to carboxyl monomer is 30:1;

[0044] When the weight ratio of the silane coupling agent to the isocyanate crosslinking agent is 1-2:2-3, the colloid has both excellent adhesion and high temperature resistance. This is because the silane coupling agent can form a Si-O-Si cross-linked network with a large bond energy between polymer molecular chains, and change the molecular chain of the acrylic polymer from a linear to a three-dimensional cross-linked network structure. Therefore, when the adhesive layer is decomposed by heat, the de-crosslinking speed slows down, thereby improving the thermal stability of the adhesive layer. However, as the amount of silane coupling agent added increases, the bonding force will weaken. It is speculated that on the one hand, the acidic environment of emulsion polymerization promotes the hydrolysis reaction of the silane coupling agent (cross-linking reaction will occur even when the silane coupling agent is added in a small amount), and the -Si(OR)3 group on the corresponding macromolecular side chain will quickly hydrolyze into -Si(OH)3, which will form a cross-linked network structure after dehydration and polycondensation, making the entanglement density of the copolymer too large, and the cohesive energy of the adhesive layer too large, which is manifested as the difficulty of the adhesive layer in wetting the surface of the bonded substrate, resulting in a decrease in the interfacial tensile failure stress and interfacial adhesion work, and a decrease in bonding force; on the other hand, as the amount of silane coupling agent added increases, the silicone will migrate to the surface of the film after curing, causing the surface energy of the film to drop too much, resulting in a decrease in bonding force. Adding a certain proportion of isocyanate cross-linking agent can improve the adhesion of the adhesive layer while maintaining a high thermal stability. It is speculated that this is because the -NCO group in the isocyanate cross-linking agent and the -OH group in the adhesive layer can form a cross-linking network more quickly, regulate the network density of the polymer more quickly, and limit the movement of silicone to the surface of the film after curing, so that the adhesive layer can achieve excellent adhesion and high temperature resistance.

[0045] Preferably, the weight ratio of the silane coupling agent to the isocyanate crosslinking agent is 1:2-2:3;

[0046] Further preferably, the weight ratio of the silane coupling agent to the isocyanate crosslinking agent is 1:1;

[0047] When the weight ratio of hydroxyl monomer, carboxyl monomer and aromatic monomer is 1-2:10:2-4, the colloid adhesion, peel strength and cohesion all achieve relatively excellent performance. Therefore, when preparing acrylic pressure-sensitive adhesive, usually the main monomer is flexible monomer, and a certain amount of aromatic hard monomer is added to increase its glass transition temperature, thereby giving the colloid sufficient cohesive strength, which can not only improve the cohesive force of the colloid, but also significantly improve the transparency and bonding strength of the film. Make the prepolymer have a sufficient degree of crosslinking, thereby improving its bonding performance, thermal stability and creep resistance. The degree of crosslinking usually needs to be controlled within a suitable range. If the degree of crosslinking is too large, the colloid adhesion will decrease. The introduction of hydroxyl groups in the acrylic pressure-sensitive adhesive system and the addition of a small amount of hydroxyl and carboxyl groups are conducive to the full play of hydrogen bonds in the system, and the additional intermolecular forces that can be provided can improve the bonding performance and peel strength of the pressure-sensitive adhesive. However, the introduction of too many active groups such as carboxyl groups will increase the amount of residual carbonyl groups in the colloid, and corrosion will occur at the bonding interface.

[0048] Preferably, the weight ratio of the hydroxyl monomer, carboxyl monomer and aromatic monomer in the modified acrylic acid ester is 1-2:10:2-4;

[0049] Further preferably, the weight ratio of the hydroxyl monomer, carboxyl monomer and aromatic monomer in the modified acrylic ester is 1:10:2;

[0050] When the weight ratio of methyl methacrylate and 4-hydroxybutyl methacrylate glycidyl ether monomers is 10:1-2, the colloid has excellent anti-warping performance. Since the glass transition temperatures of the two monomers are close and they have good compatibility, the three-dimensional network active groups formed during the curing process are evenly distributed. 4-hydroxybutyl methacrylate glycidyl ether has two active functional groups, hydroxyl and epoxy. Since the epoxy group is a rigid group, the mixed double cross-linked network formed after curing significantly increases its cohesion. At the same time, because the methacrylate glycidyl molecule also has active hydroxyl groups, it hydrogen bonds with the carboxyl groups on the polymer side chains, making the molecular arrangement more dense. The synergistic effect of covalent and physical interactions increases the cohesion, further improving the high temperature resistance of the colloid.

[0051] Preferably, the weight ratio of methyl methacrylate to 4-hydroxybutyl methacrylate glycidyl ether monomers is 10:1-2;

[0052] Further preferably, the weight ratio of methyl methacrylate to 4-hydroxybutyl methacrylate glycidyl ether monomers is 10:1;

[0053] The second aspect of the present invention provides a method for preparing a protective blue film adhesive layer for a power battery, comprising at least the following steps:

[0054] S1, in a four-necked flask, equipped with a speed-adjustable stirrer, a thermometer and a condenser, add deionized water and all emulsifiers at 25-35°C and stir and mix thoroughly for 15-25 minutes. Add weighed methyl methacrylate, butyl acrylate and modified acrylate monomers and stir until the solution is not separated. Pre-emulsify for 20-30 minutes to prepare a stable pre-emulsion A, and place at room temperature for use;

[0055] S2, install a stirring paddle, thermometer, burette, and condenser on a four-necked flask, add deionized water at 25-35°C, add initiator, oxidant, reductant, and pH buffer NaHCO, set the stirring speed to about 230-450r / min, and stir thoroughly for 10-20min. Raise the temperature to 65-70°C, start to slowly add pre-emulsion A, control the addition time to 3-3.5h, and pay attention to maintaining the stirring speed unchanged. After the pre-emulsion is added, the temperature is raised to 75-85°C, and stirring is stopped after 30-50min. Keep warm for 1.5-2.5h, stop stirring, cool, and thicken with ammonia water to prepare emulsion B;

[0056] S3, adding a silane coupling agent, an isocyanate crosslinking agent and a tackifying resin to the emulsion B at 35-45° C., stirring for 5-10 minutes, to obtain the adhesive layer.

[0057] Preferred:

[0058] S1, in a four-necked flask, equipped with a speed-adjustable stirrer, a thermometer and a condenser, add deionized water and all emulsifiers at 25°C and stir thoroughly for 15 minutes. Add weighed methyl methacrylate, butyl acrylate and modified acrylate monomers and stir until the solution is not separated. Pre-emulsify for 30 minutes to prepare a stable pre-emulsion A, and place at room temperature for use;

[0059] S2, install a stirring paddle, a thermometer, a burette, and a condenser on a four-necked flask, add deionized water at 25°C, add an initiator, an oxidant, a reductant, and a pH buffer, set the stirring speed to about 350r / min, and stir thoroughly for 15 minutes. Raise the temperature to 70°C, start to slowly drip pre-emulsion A, control the dripping time to 3h, and pay attention to maintaining the stirring speed unchanged. After the pre-emulsion is added, the temperature is raised to 80°C, and stirring is stopped after 40 minutes. Keep warm for 2h, stop stirring, cool, and thicken with ammonia water to prepare emulsion B;

[0060] S3, adding a silane coupling agent, an isocyanate crosslinking agent and a tackifying resin to the emulsion B at 40° C. and stirring for 8 minutes to obtain the adhesive layer.

[0061] Preferably, the method for preparing the blue protective film comprises the following steps:

[0062] Step (1), coating a first adhesive layer of 25-30 μm on one side of the first substrate layer, and drying at 100-110°C

[0063] After 3-7 minutes, a release film layer is attached to the first adhesive layer to form a first semi-finished product;

[0064] Step (2), coating a 25-30 μm second adhesive layer on one side of the second substrate layer, drying at 100-110° C. for 3-7 minutes, and then laminating the non-adhesive surface of the first substrate layer of the first semi-finished product on the second adhesive layer to form a second semi-finished product;

[0065] Step (3), the second semi-finished product is aged at 45-55° C. for 40-48 hours to obtain a blue film;

[0066] The preparation of the blue film also includes step (4), dividing the blue film into strips of different widths according to customer requirements.

[0067] The lamination conditions include a temperature of 45-55° C. and a pressure of 0.4-0.6 MPa.

[0068] Beneficial effects:

[0069] 1. When the weight ratio of methyl methacrylate to terpene resin is 3-4:1, it can not only change the internal structure of the colloid, but also improve its surface properties, so that the polymer has excellent adhesion and achieves a technical effect that is conducive to processing.

[0070] 2. When the weight ratio of methyl methacrylate and 4-hydroxybutyl methacrylate glycidyl ether monomers is 10:1-2, the colloid has excellent anti-warping performance. Since the glass transition temperatures of the two monomers are close and they have good compatibility, the three-dimensional network active groups formed during the curing process are evenly distributed. 4-hydroxybutyl methacrylate glycidyl ether has two active functional groups, hydroxyl and epoxy. Since the epoxy group is a rigid group, the mixed double cross-linked network formed after curing significantly increases its cohesion. At the same time, because the methacrylate glycidyl molecule also has active hydroxyl groups, it hydrogen bonds with the carboxyl groups on the polymer side chains, making the molecular arrangement more dense. The synergistic effect of covalent and physical interactions increases the cohesion, further improving the high temperature resistance of the colloid.

[0071] 3. When the weight ratio of methyl methacrylate to acrylic acid is 30:0.5-1, the colloid has both excellent adhesion and anti-warping performance. The reason is that the acrylic acid molecule carries a polar functional group carboxyl group, and the active hydrogen atom in the carboxyl group can form a hydrogen bond with the ester group on the copolymer molecular chain segment, thereby enhancing the intermolecular force, thereby enhancing the adhesion and anti-warping performance of the colloid.

[0072] 4. When the weight ratio of silane coupling agent to isocyanate crosslinking agent is 1-2:2-3, the colloid has both excellent bonding and high temperature resistance. This is because the silane coupling agent can form a Si-O-Si crosslinking network with a large bond energy between polymer molecular chains. When thermally decomposed, the de-crosslinking speed of the adhesive layer slows down, thereby improving the thermal stability of the adhesive layer. However, as the amount of silane coupling agent added increases, the bonding strength will weaken. Adding a certain proportion of isocyanate crosslinking agent can keep the adhesive layer at a high thermal stability while improving the bonding strength of the adhesive layer, so that the adhesive layer has both excellent bonding and high temperature resistance.

[0073] 5. When the weight ratio of hydroxyl monomer, carboxyl monomer and aromatic monomer is 1-2:10:2-4, the colloid adhesion, peel strength and cohesion all achieve relatively excellent performance. Therefore, when preparing acrylic pressure-sensitive adhesive, usually the flexible monomer is mainly used, and a certain amount of aromatic hard monomer is added to increase its glass transition temperature, thereby giving the colloid sufficient cohesion strength, which can not only improve the cohesion of the colloid, but also significantly improve the transparency and bonding strength of the film. The introduction of hydroxyl groups in the acrylic pressure-sensitive adhesive system and the addition of a small amount of hydroxyl and carboxyl groups are conducive to the full play of hydrogen bonds in the system, and the additional intermolecular forces can improve the adhesion and peel strength of the pressure-sensitive adhesive. However, the introduction of too many active groups such as carboxyl groups will increase the amount of residual carbonyl groups in the colloid, and corrosion will occur at the bonding interface. Therefore, when the weight ratio of hydroxyl monomer, carboxyl monomer and aromatic monomer is 1-2:10:2-4, the colloid adhesion, peel strength and cohesion performance are balanced. DETAILED DESCRIPTION

[0074] Example 1

[0075] A protective blue film for a power battery, characterized in that the blue film comprises: a substrate layer, a glue layer and a release film layer:

[0076] The adhesive layer includes a first adhesive layer and a second adhesive layer;

[0077] The substrate layer includes a first substrate layer and a second substrate layer;

[0078] The structure of the blue film, from inside to outside, is the second substrate layer, the second adhesive layer, the first substrate layer, the first adhesive layer, and the release film layer;

[0079] The adhesive layer is a methacrylate copolymer with a weight average molecular weight of 130±100,000;

[0080] The release film layer material is selected from polyethylene terephthalate, has a thickness of 25 μm, and is purchased from Suzhou Chenfan New Materials Co., Ltd.;

[0081] The substrate layer material is PET, purchased from Dongwan Zhonglian Electronic Materials Co., Ltd., with a thickness of 25 μm;

[0082] The first adhesive layer and the second adhesive layer have the same composition;

[0083] The coating thickness of the adhesive layer is 30 μm;

[0084] A protective blue film for a power battery, the adhesive layer includes the following raw materials in parts by weight: 36 parts of methyl methacrylate; 15 parts of butyl acrylate; 14 parts of modified acrylic resin; 12 parts of tackifying resin; 1 part of silane coupling agent; 1 part of isocyanate crosslinking agent; 0.5 parts of initiator; 4 parts of dye; 1 part of buffer; 3 parts of emulsifier; 1 part of oxidant; 1 part of reducing agent; 2 parts of pH regulator; 100 parts of deionized water;

[0085] The modified acrylic resin comprises, by weight, hydroxyl monomer: 1 part of 4-hydroxybutyl methacrylate glycidyl ether; carboxyl monomer: 10 parts of acrylic acid; aromatic monomer: 2 parts of phenyl methacrylate;

[0086] The emulsifier is sodium dodecylbenzene sulfonate (CAS No.: 25155-30-0);

[0087] The buffer is 0.5 mol / L sodium bicarbonate solution (CAS No.: 144-55-8);

[0088] The initiator is ammonium persulfate (CAS No.: 7727-54-0);

[0089] The oxidant is tert-butyl hydroperoxide (CAS No.: 75-91-2);

[0090] The reducing agent is sodium formaldehyde sulfoxylate (CAS No.: 870-72-4);

[0091] The pH regulator is aqueous ammonia containing 27% ammonia;

[0092] The dye was purchased from indigo dye produced by Yizhou Textile Dyeing Company, model number CFX-1;

[0093] The tackifying resin is purchased from the terpene resin of Jinlin Chemical, model number is T100;

[0094] The alkane coupling agent is γ-aminopropyltrimethoxysilane (CAS No.: 13822-56-5);

[0095] The isocyanate cross-linking agent is isophorone diisocyanate (CAS No.: 4098-71-9);

[0096] A method for preparing a protective blue film adhesive layer for a power battery comprises the following steps:

[0097] S1, in a four-necked flask, equipped with a speed-adjustable stirrer, a thermometer and a condenser, add deionized water and all emulsifiers at 25°C and stir thoroughly for 15 minutes. Add weighed methyl methacrylate, butyl acrylate and modified acrylate monomers and stir until the solution is not separated. Pre-emulsify for 30 minutes to prepare a stable pre-emulsion A, and place at room temperature for use;

[0098] S2, install a stirring paddle, a thermometer, a burette, and a condenser on a four-necked flask, add deionized water at 25°C, add an initiator, an oxidant, a reductant, and a pH buffer, set the stirring speed to about 350r / min, and stir thoroughly for 15 minutes. Raise the temperature to 70°C, start to slowly drip pre-emulsion A, control the dripping time to 3h, and pay attention to maintaining the stirring speed unchanged. After the pre-emulsion is added, the temperature is raised to 80°C, and stirring is stopped after 40 minutes. Keep warm for 2h, stop stirring, cool, and thicken with ammonia water to prepare emulsion B;

[0099] S3, adding a silane coupling agent, an isocyanate crosslinking agent and a tackifying resin to the emulsion B at 40° C. and stirring for 8 minutes to obtain the adhesive layer.

[0100] A method for preparing a protective blue film for a power battery comprises the following steps:

[0101] Step (1), coating a first adhesive layer of 25 μm on one side of the first substrate layer, drying at 110° C. for 5 min, and then laminating a release film layer on the first adhesive layer to form a first semi-finished product;

[0102] Step (2), coating a 25 μm second adhesive layer on one side of the second substrate layer, drying at 110° C. for 5 min, and laminating the non-adhesive surface of the first substrate layer of the first semi-finished product on the second adhesive layer to form a second semi-finished product;

[0103] Step (3), the second semi-finished product is cured at 50° C. for 48 hours to obtain a blue film;

[0104] The lamination conditions are a temperature of 50° C. and a pressure of 0.5 MPa.

[0105] Example 2

[0106] The specific implementation is the same as in Example 1; the difference is that in Example 2, the amount of methyl methacrylate is 40 parts.

[0107] Example 3

[0108] The specific implementation is the same as in Example 1; the difference is that the weight portion of isophorone diisocyanate in Example 3 is 2 parts.

[0109] Comparative Example 1

[0110] Specific implementation method is the same as Example 1; the difference is that the weight parts of the carboxyl monomer in Comparative Example 1 is 15 parts.

[0111] Comparative Example 2

[0112] The specific implementation method is the same as Example 1; the difference is that the hydroxyl monomer in the modified acrylic ester of Comparative Example 2 is hydroxypropyl methacrylate (CAS No.: 27813-02-1);

[0113] Comparative Example 3

[0114] The specific implementation is the same as Example 1; the difference is that the number of aromatic monomers in the modified acrylic ester in Comparative Example 3 is 5 parts.

[0115] Comparative Example 4

[0116] The specific implementation is the same as Example 1; the difference is that in Comparative Example 4, the amount of methyl methacrylate is 30 parts.

[0117] Performance Testing Methods

[0118] 1. Warpage resistance: No residual glue or warping at 25℃ for 24 hours;

[0119] 2. High temperature resistance: After the aluminum shell is attached, it is kept at 85℃ for 4 hours without residual glue or warping;

[0120] 3. Flame retardant performance: HB for horizontal combustion and V2 for vertical combustion (with 1mm aluminum plate) as specified by UL94 standard;

[0121] 4. Insulation performance: Test at a temperature of 23±2℃ and a humidity of 55±5% for 2 hours, then use a high voltage of 1000V / 50hz for 1 minute, and observe the appearance of the tape. It must not be damaged or punctured;

[0122] Performance test data

[0123]

[0124]

Claims

1. A protective blue film for a power battery, characterized in that: The blue film comprises: a substrate layer, an adhesive layer and a release film layer: The adhesive layer includes a first adhesive layer and a second adhesive layer; The substrate layer includes a first substrate layer and a second substrate layer; The structure of the blue film, from inside to outside, is the second substrate layer, the second adhesive layer, the first substrate layer, the first adhesive layer, and the release film layer; The adhesive layer is a methacrylate copolymer with a weight average molecular weight of 1-1.5 million; The release film layer material is selected from one of polypropylene, polyimide, and polyethylene terephthalate; The substrate layer is a PET film with a thickness of 20-30 μm; The first adhesive layer and the second adhesive layer have the same composition; The coating thickness of the adhesive layer is 25-30 μm; The adhesive layer includes the following raw materials in parts by weight: 35-40 parts of methyl methacrylate, 15-25 parts of butyl acrylate, 10-15 parts of modified acrylic ester monomers, 10-15 parts of tackifying resins, 1-4 parts of silane coupling agents, 1-4 parts of isocyanate crosslinking agents, 0.5-1 parts of initiators, 1-10 parts of dyes, 1-2 parts of buffers, 3 parts of emulsifiers, 1-2 parts of oxidants, 1-2 parts of reducing agents, 2-3 parts of pH regulators, and 100 parts of deionized water; The modified acrylic resin comprises: a hydroxyl monomer, a carboxyl monomer and an aromatic monomer; the hydroxyl monomer is 4-hydroxybutyl methacrylate glycidyl ether; the carboxyl monomer is acrylic acid; and the aromatic monomer is phenyl methacrylate; The tackifying resin in the adhesive layer raw material is selected from terpene resin, and the weight ratio of methyl methacrylate to terpene resin is 3-4:1; The weight ratio of the hydroxyl monomer, the carboxyl monomer and the aromatic monomer in the modified acrylic ester is 1-2:10:2-4.

2. A protective blue film for power batteries according to claim 1, characterized in that: The weight ratio of the silane coupling agent to the isocyanate crosslinking agent in the colloidal raw material is 1:

1.

3. A protective blue film for a power battery according to claim 1, characterized in that: The weight ratio of methyl methacrylate to carboxyl monomer in the colloid raw material is 30:0.5-1.

4. A protective blue film for a power battery according to any one of claims 1 to 3, characterized in that: The method for preparing the adhesive layer comprises at least the following steps: S1, weigh 35-40 parts of methyl methacrylate, 15-25 parts of butyl acrylate, 10-15 parts of modified acrylic ester monomer, 10-15 parts of tackifying resin, 1-4 parts of silane coupling agent, 1-4 parts of isocyanate crosslinking agent, and 0.5-1 parts of initiator by weight; S2, add deionized water and all emulsifiers at 25-35°C and stir and mix thoroughly for 15-25 minutes; add weighed methyl methacrylate, butyl acrylate and modified acrylate monomers and stir until the solution is not separated; pre-emulsify for 20-30 minutes to prepare a stable pre-emulsion A, and place at room temperature for use; S3, add deionized water at 25-35°C, add initiator, oxidant, reductant and pH buffer at the same time, set the stirring speed to 230-450r / min, and stir thoroughly for 10-20min; raise the temperature to 65-70°C, start to slowly drip pre-emulsion A, control the dripping time to 3-3.5h, and pay attention to maintain the stirring speed unchanged; after the pre-emulsion is dripped, the temperature is raised to 75-85°C, and the stirring is stopped after 30-50min, and the temperature is kept for 1.5-2.5h, and the stirring is stopped. After cooling, the emulsion is thickened with ammonia water to prepare emulsion B; S4, adding a silane coupling agent, an isocyanate crosslinking agent and a tackifying resin to the emulsion B at 35-45° C., stirring for 5-10 minutes, to obtain the adhesive layer.

5. A method for preparing a protective blue film for a power battery according to claim 4, characterized in that: At least the following steps are included: Step (1), coating a first adhesive layer on one side of the first substrate layer, and after drying, laminating a release film layer on the first adhesive layer to form a first semi-finished product; Step (2), coating a second adhesive layer on one side of the second substrate layer, and after drying, laminating the non-adhesive surface of the first substrate layer of the first semi-finished product on the second adhesive layer to form a second semi-finished product; Step (3), the second semi-finished product is ripened to obtain a blue film.

6. The method for preparing a protective blue film for a power battery according to claim 5, characterized in that: The drying temperature is 100-110°C.

Citation Information

Patent Citations

  • High temperature-resistant and UV (Ultraviolet)-resistant protective film and preparation method thereof

    CN108707432A

  • Acrylate adhesive, adhesive tape and preparation method thereof

    CN114752323A

  • Organic silicon modified phenyl emulsion pressure-sensitive adhesive with high release force and low residue as well as preparation method thereof and application

    CN104342073A

  • Blue film adhesive tape for square lithium battery cell

    CN215560039U