A COFs nanomaterial mixed matrix ultrafiltration membrane based on Teregu base and preparation method thereof
By preparing ultrafiltration membranes by blending Teleg base COF nanomaterials with polysulfone polymers, the problem of high cost of low molecular weight ultrafiltration membranes in existing technologies is solved, achieving low-cost, high-efficiency separation of low molecular weight proteins and multiple uses.
Patent Information
- Application Number
- CN202211641623.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-20
AI Technical Summary
Currently, ultrafiltration membrane materials with low molecular weight rejection rates rely on imports. The synthesis process is complex and costly, making it difficult to meet the high-efficiency separation requirements of low molecular weight proteins in biomedicine.
A mixed-matrix ultrafiltration membrane was prepared by blending Teleg base COF nanomaterials with polysulfone polymers and using a solvent-inducible phase separation technique. The membrane pore size was adjusted to improve the retention performance of low molecular weight proteins.
It achieves low-cost, high-efficiency separation of low molecular weight proteins. The membrane material can be recycled multiple times without secondary pollution and is suitable for screening and concentrating proteins of different molecular weights.
Smart Images

Figure CN115845616B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of membrane separation, and in particular relates to a COFs nanomaterial mixed matrix ultrafiltration membrane based on a Tetragol base and a preparation method thereof. Background Art
[0002] Membrane separation technology is the most widely used and most promising separation and purification technology today. The membrane separation process has the characteristics of no phase change, low energy consumption, high separation selectivity, simple process, and easy operation. It is widely used in food, medicine, biology, chemical production, sewage treatment, and seawater desalination. According to the different operating modes, it can be divided into pressure-driven membranes, electrically driven membranes, etc. Among them, according to the membrane pore size and separation ability, the pressure-driven membrane can be divided into microfiltration membrane (MF), ultrafiltration membrane (UF), nanofiltration membrane (NF) and reverse osmosis membrane (RO). The pore size range of ultrafiltration membranes is generally 5nm to 100nm, and it is mainly used to retain molecular weight greater than 1000g·mol -1 of substance.
[0003] At present, the methods commonly used for protein separation and purification in biomedicine are mostly physical and chemical methods such as precipitation, salting out, chromatography, continuous centrifugation, filtration or extraction. Continuous centrifugation and chromatography technology are still widely used in protein separation, but the protein molecules obtained by simple separation in the past generally have disadvantages such as low purity and complex operation; and chemical purification methods such as precipitation, salting out, extraction, etc. are easily destroyed when purifying some biologically active or heat-sensitive substances. Ultrafiltration technology is a biological separation and purification technology that is currently widely used. The use of ultrafiltration centrifugation can achieve the screening, purification and concentration of protein molecules of different molecular weights in a relatively short time. At present, there is a large demand for ultrafiltration membranes with low molecular weight cutoff rates in China, but most membrane materials rely on imports, the synthesis process is complicated, and the cost is high. Therefore, it is of great practical significance to develop a low-cost, low molecular weight cutoff ultrafiltration membrane. Summary of the invention
[0004] The purpose of the present invention is to address the shortcomings of the current domestic low molecular weight retention rate ultrafiltration membrane preparation technology, and propose a mixed matrix ultrafiltration membrane based on COFs nanomaterials as a blending material and a preparation method thereof. The ultrafiltration membrane prepared by the invention can achieve the separation of low molecular weight proteins.
[0005] In order to achieve the above object, the present invention implements the following technical solutions:
[0006] A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu bases comprises the following steps:
[0007] 1) taking a Teregu base monomer with primary amine groups at both ends in water, adding glacial acetic acid to adjust the pH to obtain solution A; taking trialdehyde phloroglucinol or pyromellitic trimesic acid in an organic solvent, stirring evenly to obtain solution B;
[0008] 2) Mixing solution A and solution B, stirring evenly, and standing to react to generate COFs nanomaterials to obtain suspension C;
[0009] 3) After the suspension C is allowed to settle, it is centrifuged and the precipitate is retained; the precipitate is repeatedly washed and dried to obtain COFs powder;
[0010] 4) preparing a casting solution: weighing a certain amount of COFs powder and dissolving it in an organic solvent, crushing and dispersing it by ultrasonication to obtain a homogeneous solution, and then weighing a certain amount of polysulfone substrate and porogen and adding them to the homogeneous solution to obtain a casting solution; heating and stirring the obtained casting solution at a certain temperature until it is completely dissolved, and continuing to heat the casting solution after it is stirred and mixed evenly, and standing to degas;
[0011] 5) Preparation of ultrafiltration membrane: pour the completely degassed casting liquid onto a glass plate carrier with non-woven fabric, use a scraper to evenly spread the casting liquid on the surface of the non-woven fabric, and immediately put it into a pure water bath to solidify into a membrane; then soak the prepared membrane in ultrapure water.
[0012] In step 1), the Teregu base monomer with primary amine groups at both ends is TBDA, and the structural formulas of TBDA, TP and TBA are as follows:
[0013]
[0014] In step 1), after the Teleg base monomer with primary amine groups at both ends is dissolved in water, the solute concentration in the solution is 2.8-3.1wt%; glacial acetic acid is used to adjust the pH to 3; the solute concentration in solution B is 2.1-2.5wt%; and the organic solvent is one of acetonitrile, dichloroethane, cyclohexane, n-hexane, and n-heptane.
[0015] In step 2), solution A and solution B are mixed in a mass ratio of 1:0.75-1.5.
[0016] The reaction equations for preparing COFs nanomaterials in step 2) are:
[0017]
[0018]
[0019] In step 4), the mass fraction of the polysulfone substrate in the casting solution is 15% to 30%, the mass fraction of the COFs nanomaterial in the casting solution is 1% to 20%, the mass fraction of the porogen in the casting solution is 1% to 10%, and the mass fraction of the organic solvent in the casting solution is 50% to 80%.
[0020] In step 4), the polysulfone substrate is polysulfone or polyethersulfone; the porogen is one or more of PVPK15, PVPK25, PVPK30, PVPK60, PF127, PEG 300, PEG 600, PEG 2000, PEG 4000 and LiCl.
[0021] In step 4), the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and dimethyl sulfoxide.
[0022] In step 5), the thickness of the scraper is 100 μm to 250 μm; the temperature during film scraping is 20° C. to 70° C.
[0023] The temperature of the pure water bath in step 5) is 0°C to 30°C.
[0024] The beneficial effects of the present invention are as follows: the present invention prepares a mixed matrix ultrafiltration membrane for retaining low molecular weight proteins by blending COFs nanomaterials, and can achieve the retention effect for proteins of different molecular weights by parameters such as conditional casting liquid and scraping conditions, and adjusts the pore size of the ultrafiltration membrane based on the good compatibility between the COFs nanomaterials and the polysulfone polymers, thereby improving the retention performance of the ultrafiltration membrane for proteins; the product is prepared by adopting a non-solvent-induced phase separation technology, the membrane preparation process is low in difficulty and production cost, the ultrafiltration membrane can be recycled and reused multiple times, there is no secondary pollution, and the product has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a comparison diagram of the ultrafiltration membrane (a) prepared in Example 1 of the present invention and the ultrafiltration membrane (b) prepared in Comparative Example 1. DETAILED DESCRIPTION
[0026] The following is a further detailed description in conjunction with specific embodiments to make the content of the invention more clear, but the content and scope of the invention are not limited to the following embodiments, and normal variations thereof should all fall within the scope of the invention.
[0027] Embodiment 1:
[0028] Step 1: Take a Teregulin base monomer (TBDA) with primary amine groups at both ends and dissolve it in water to prepare a solution with a concentration of 2.8wt%, add glacial acetic acid to adjust the pH to 3, and obtain solution A; take trialdehyde phloroglucinol (TP) in acetonitrile and stir evenly to obtain a solution B with a concentration of 2.1wt%.
[0029] Step 2: Mix solution A and solution B in a mass ratio of 1:1, stir evenly, and let stand for half an hour to react to obtain suspension C.
[0030] Step 3: After the suspension C is allowed to stand and precipitate, the precipitate is retained by centrifugation; the precipitate is washed with ethanol and dried in a vacuum oven, and COFs powder is obtained after repeated washing and drying.
[0031] Step 4: Prepare casting solution: Weigh a certain amount of COFs powder and dissolve it in N,N-dimethylformamide solvent, crush and disperse it by ultrasonication to obtain a homogeneous solution, and then weigh a certain amount of polyethersulfone PES and PVP K60 and add them to the above homogeneous solution to obtain casting solution. The obtained casting solution is heated and stirred at a certain temperature until it is completely dissolved. After the casting solution is stirred and mixed evenly, continue to heat it and stand it for degassing. The mass ratios of PES, COFs, PVP K60 and N,N-dimethylformamide are 16%, 0.5%, 3.5% and 80%.
[0032] Step 5: Preparation of ultrafiltration membrane: Pour the completely degassed casting solution onto a glass plate carrier with non-woven fabric, use a 250μm scraper to evenly spread the casting solution on the surface of the non-woven fabric (control the temperature at 20℃~70℃ when scraping the membrane), and immediately put it into a pure water bath (control the temperature at 0℃~30℃) to solidify into a membrane. The prepared membrane is soaked in ultrapure water.
[0033] Embodiment 2, 3:
[0034] The experimental process for preparing mixed matrix ultrafiltration membranes in Examples 2 and 3 was repeated in Example 1, except that in step 4, the mass ratios of PES, COFs, PVP K30 and N,N-dimethylformamide were 19%, 0.5%, 3.5%, 77%; and 21%, 0.5%, 3.5%, 75%, respectively.
[0035] Comparative Example 1:
[0036] Step 1: Prepare casting solution: Weigh a certain amount of PES and PVP K60 and add them to N,N-dimethylformamide solvent to obtain casting solution. The obtained casting solution is heated and stirred at a certain temperature until it is completely dissolved. After the casting solution is stirred and mixed evenly, continue to heat it and stand it for degassing. The mass ratios of PES, PVP K60 and N,N-dimethylformamide are 16%, 0.5%, 3.5% and 80%.
[0037] Step 2: Preparation of ultrafiltration membrane: Pour the completely degassed casting solution onto a glass plate carrier with non-woven fabric, use a scraper to evenly spread the casting solution on the surface of the non-woven fabric, and immediately put it into a pure water bath to solidify into a membrane. The prepared membrane is soaked in ultrapure water.
[0038] Comparative Examples 2 and 3: The experimental process for preparing mixed matrix ultrafiltration membranes was repeated in Comparative Example 1, except that in step 4, the mass ratios of PES, PVP K60 and N,N-dimethylformamide were 19%, 0.5%, 3.5%, 77%; 21%, 0.5%, 3.5%, 75%.
[0039] Performance evaluation:
[0040] The mixed matrix ultrafiltration membrane doped with COFs nanospheres prepared in each embodiment is combined with a special centrifuge tube to form an ultrafiltration centrifuge tube for performance testing. A centrifuge with a fixed angle rotor is used, and the prepared test centrifuge tube is placed in a centrifuge and operated for 20 minutes at a centrifugal force of 5000xg (about 7441r / min). Among them, the test substances are bovine serum albumin (BSAMw67000), pepsin (Pepsin Mw34500), lysozyme (Lysozyme Mw14500), dextran 20000 (Dextran20000), dextran 10000 (Dextran10000), polyethylene glycol 8000 (PEG8000), polyethylene glycol 6000 (PEG6000), etc.
[0041] Table 1 Performance evaluation of ultrafiltration membranes prepared in different examples
[0042]
[0043] By comparing Examples 1-3 with Comparative Examples 1-3, it can be seen that the mixed matrix membrane prepared using COFs nanomaterials can effectively improve the retention capacity of the ultrafiltration membrane for substances with different molecular weights.
[0044] Embodiment 4:
[0045] Step 1: Take a Teregu base monomer (TBDA) with primary amine groups at both ends and dissolve it in water to prepare a solution with a concentration of 3.1wt%, add glacial acetic acid to adjust the pH to 3, and obtain solution A; take trimesaldehyde (TBA) in cyclohexane and stir evenly to obtain a solution B with a concentration of 2.5wt%.
[0046] Step 2: Mix solution A and solution B in a mass ratio of 1:1.1, stir evenly, and let stand to react for one hour to obtain suspension C.
[0047] Step 3: After the suspension C is allowed to stand and precipitate, the precipitate is retained by centrifugation; the precipitate is washed with ethanol and dried in a vacuum oven, and COFs powder is obtained after repeated washing and drying.
[0048] Step 4: Prepare casting solution: Weigh a certain amount of COFs powder and dissolve it in N,N-dimethylformamide solvent, crush and disperse it by ultrasonication to obtain a homogeneous solution, and then weigh a certain amount of PES and PEG600 and add them to the above homogeneous solution to obtain casting solution. The obtained casting solution is heated and stirred at a certain temperature until it is completely dissolved. After the casting solution is stirred and mixed evenly, continue to heat it and stand it for degassing. The mass ratios of PES, COFs, PEG600 and N,N-dimethylformamide are 15%, 0.8%, 8.2% and 76%.
[0049] Step 5: Preparation of ultrafiltration membrane: Pour the completely degassed casting solution onto a glass plate carrier with non-woven fabric, use a 100 μm scraper to evenly spread the casting solution on the surface of the non-woven fabric (control the temperature at 20°C to 70°C when scraping the membrane), and immediately put it into a pure water bath (control the temperature at 0°C to 30°C) to solidify into a membrane. The prepared membrane is soaked in ultrapure water.
[0050] Embodiment 5, 6:
[0051] The experimental process for preparing mixed matrix ultrafiltration membranes in Examples 2 and 3 was repeated in Example 4, except that in step 4, the mass ratios of PES, COFs, PEG600 and N,N-dimethylformamide were 17.5%, 0.8%, 8.2%, 73.5%; 21%, 0.8%, 8.2%, 70%.
[0052] Comparative Example 4:
[0053] Step 1: Prepare casting solution: Weigh a certain amount of PES and PEG600 and add them to N,N-dimethylformamide solvent to obtain casting solution. The obtained casting solution is heated and stirred at a certain temperature until it is completely dissolved. After the casting solution is stirred and mixed evenly, it is continued to be heated and allowed to stand for degassing. The mass ratios of PES, PEG600 and N,N-dimethylformamide are 15%, 8.2% and 76% respectively.
[0054] Step 2: Preparation of ultrafiltration membrane: Pour the completely degassed casting solution onto a glass plate carrier with non-woven fabric, use a 150μm scraper to evenly spread the casting solution on the surface of the non-woven fabric, and immediately put it into a pure water bath to solidify into a membrane. The prepared membrane is soaked in ultrapure water.
[0055] Comparative Examples 5 and 6: The experimental process for preparing mixed matrix ultrafiltration membranes was repeated in Comparative Example 4, except that in step 4, the mass ratios of PES, PEG600 and N,N-dimethylformamide were 17.5%, 8.2%, 73.5%; 21%, 8.2%, 70%.
[0056] Performance evaluation:
[0057] Performance evaluation of Examples 4-6 and Comparative Examples 4-6 (same experimental process as that of Examples 1-3 and Comparative Examples 1-3).
[0058] Table 2 Performance evaluation of ultrafiltration membranes prepared in different examples
[0059]
[0060] By comparing Examples 4-6 with Comparative Examples 4-6, it can be seen that the mixed matrix membrane prepared using COFs nanomaterials can effectively improve the retention capacity of the ultrafiltration membrane for substances with different molecular weights.
[0061] In the present invention, in step 1), when preparing solution B, the organic solvent used can also be one of dichloroethane, n-hexane, and n-heptane. In step 2), solution A and solution B can be mixed at a mass ratio of 1:0.75-1.5 to obtain COFs nanomaterials. Step 4) When preparing the casting solution, the COFs powder can also be dissolved in one or more solvents selected from N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and dimethyl sulfoxide; the polysulfone substrate can also be polysulfone; in addition to the above-mentioned PVP K60 and PEG 600, the porogen can also be one or more of PVP K15, PVP K25, PVP K30, PVP K60, PEG600, PF127, PEG 300, PEG 2000, PEG 4000 and LiCl; based on the requirements for the retention effect of proteins with different molecular weights, the casting solution can be prepared as follows: the mass fraction of the polysulfone substrate in the casting solution is 15% to 30%, the mass fraction of the COFs nanomaterial in the casting solution is 1% to 20%, the mass fraction of the porogen in the casting solution is 1% to 10%, and the mass fraction of the organic solvent in the casting solution is 50% to 80%.
[0062] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base, It is characterized in that The following steps are involved: 1) taking a Teregu base monomer with primary amine groups at both ends in water, adding glacial acetic acid to adjust the pH to obtain solution A; taking trialdehyde phloroglucinol or pyromellitic trimesic acid in an organic solvent, stirring evenly to obtain solution B; 2) Mix solution A and solution B in a mass ratio of 1:0.75-1.5, stir evenly, and allow to react to generate COFs nanomaterials to obtain suspension C; 3) After the suspension C is allowed to settle, it is centrifuged and the precipitate is retained; the precipitate is repeatedly washed and dried to obtain COFs powder; 4) preparing a casting solution: weighing a certain amount of COFs powder and dissolving it in an organic solvent, crushing and dispersing it by ultrasonication to obtain a homogeneous solution, and then weighing a certain amount of polysulfone substrate and porogen and adding them to the homogeneous solution to obtain a casting solution; heating and stirring the obtained casting solution at a certain temperature until it is completely dissolved, and continuing to heat the casting solution after it is stirred and mixed evenly, and standing to degas; 5) Preparation of ultrafiltration membrane: Pour the completely degassed casting liquid onto a glass plate carrier with non-woven fabric, use a scraper to evenly spread the casting liquid on the surface of the non-woven fabric, and immediately put it into a pure water bath to solidify into a membrane; then soak the prepared membrane in ultrapure water.
2. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base according to claim 1, It is characterized in that In step 1), the Teregu base monomer with primary amine groups at both ends is TBDA, and the structural formulas of TBDA, TP and TBA are shown below:
3. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base as claimed in claim 1, Features: In step 1), after the Teleg base monomer with primary amine groups at both ends is dissolved in water, the solute concentration in the solution is 2.8-3.1wt%; glacial acetic acid is used to adjust the pH to 3; the solute concentration in solution B is 2.1-2.5wt%; and the organic solvent is one of acetonitrile, dichloroethane, cyclohexane, n-hexane, and n-heptane.
4. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base according to claim 1, It is characterized in that The reaction equations for preparing COFs nanomaterials in step 2) are:
5. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base according to claim 1, Features: In step 4), the mass fraction of the polysulfone substrate in the casting solution is 15% to 30%, the mass fraction of the COFs nanomaterial in the casting solution is 1% to 20%, the mass fraction of the porogen in the casting solution is 1% to 10%, and the mass fraction of the organic solvent in the casting solution is 50% to 80%.
6. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base according to claim 1, Features: In step 4), the polysulfone substrate is polysulfone or polyethersulfone; the porogen is one or more of PVP K15, PVP K25, PVP K30, PVP K60, PF127, PEG 300, PEG 600, PEG 2000, PEG 4000 and LiCl.
7. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu bases as claimed in claim 1, Features: In step 4), the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and dimethyl sulfoxide.
8. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Teregu base according to claim 1, Features: In step 5), the thickness of the scraper is 100 μm to 250 μm; the temperature during film scraping is 20° C. to 70° C.
9. A method for preparing a mixed matrix ultrafiltration membrane of COFs nanomaterials based on Tereger bases as claimed in claim 1, Features: The temperature of the pure water bath in step 5) is 0°C to 30°C.