A kind of strong alkali resistant polyester resin and preparation method thereof, and strong alkali resistant powder coating

By introducing sterically hindered groups and polyfunctional alcohol end-capping and secondary vacuum processes into the polyester resin, combined with isocyanate and other materials, strong alkali-resistant polyester resins and powder coatings were prepared, which solved the problem of polyester resin in strong alkali. The problem of insufficient durability in the environment is achieved by achieving efficient strong alkali resistance.

CN115850674BActive Publication Date: 2024-10-25ANHUI SHENJIAN NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211610266.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-10-25
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

Existing polyester resins lack durability in strong alkaline environments and are prone to loss of gloss, blistering, cracking, powdering and falling off, and cannot meet the corrosion resistance requirements of high concentrations of strong alkali.

Method used

Synthetic monomers containing sterically hindered groups are used, and through multifunctional alcohol end-capping and secondary vacuum processes, the steric hindrance effect and cured cross-linking density are improved, the residual carboxyl content in the polyester resin is reduced, and the interaction with strong alkali is reduced. Reaction, and combining isocyanate, pigment, leveling agent and wetting accelerator in powder coating, and preparing strong alkali-resistant polyester resin and powder coating through twin-screw extruder.

Benefits of technology

Under the conditions of 30℃ and 60℃, after soaking in 50%wt NaOH, the gloss retention rate of the coating is greater than 75% and 60%, without cracking, powdering or falling off, significantly improving the resistance to strong alkali.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003999193620000111
    Figure BDA0003999193620000111
  • Figure BDA0003999193620000121
    Figure BDA0003999193620000121
  • Figure BDA0003999193620000131
    Figure BDA0003999193620000131
Patent Text Reader

Abstract

A kind of strong alkali resistant polyester resin and preparation method thereof, strong alkali resistant powder coating, the raw materials of the strong alkali resistant polyester resin are: 5.4-6.0 parts of polyol, 5.8-6.3 parts of polyacid, 0.05-0.35 parts of glycidyl ester, 0.008-0.012 parts of esterification catalyst, and 0.1-0.3 parts of end-capping agent. The present invention selects synthetic monomers containing steric hindrance groups, adopts multifunctional alcohols for end-capping and secondary vacuum process, effectively improves the steric hindrance effect and curing crosslinking density, and reduces the residual carboxyl content in the polyester resin to within 1mgKOH / g, reducing the reaction of carboxyl and strong alkali. The prepared polyester resin is applied to polyurethane powder coating, and the coating has good leveling, mechanical properties, adhesion, and water boiling resistance, and has excellent strong alkali resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a strong alkali-resistant polyester resin and a preparation method thereof, and a strong alkali-resistant powder coating. Background Art

[0002] The corrosion of metals in nature is mainly electrochemical corrosion. Regardless of storage or use, metal materials always come into contact with the surrounding atmosphere or certain media. The atmosphere contains elements such as hydrogen, oxygen, sulfur, and chlorine, and contains a certain amount of humidity. These elements cause differences in the pH value of humid gas, so when metal materials are used in the atmosphere, electrochemical conditions are easily formed. If used in acid, alkali, or salt media, the corrosion will be more serious.

[0003] The anti-corrosion effect of powder coating is to form a dense coating on the metal surface, preventing water, oxygen and other electrolytes from contacting the metal interior, and shielding the environment. The alkali resistance of the coating refers to the ability of the coating to resist alkali corrosion, that is, under specified conditions, the coating test plate is immersed in a certain concentration of alkali solution, and there is no loss of gloss, bubbling, whitening, falling off, etc. within the specified time.

[0004] Polyester resin contains a large number of ester bonds, which have poor alkali resistance. Among the existing polyester / TGIC, polyester / HAA, polyester / epoxy, and polyurethane powder coating systems, the polyurethane system has slightly better alkali resistance, but its coating mechanical properties and adhesion to the substrate are often poor, and it lacks durability in strong alkaline solutions. If the coating is in a strong alkaline environment for a long time, the physical and chemical structure of the coating will be destroyed, and phenomena such as gloss loss, blistering, cracking, powdering, and falling off will be more serious.

[0005] The Chinese patent "A Corrosion-Resistant Polyester Resin and Its Preparation Method" with publication number CN 111393621 A published on July 10, 2020, discloses that the raw materials of the corrosion-resistant polyester resin are: 15-20 parts of ether polyol, 20-25 parts of diol, 10-20 parts of multifunctional acid or multifunctional acid anhydride, 35-60 parts of dibasic acid or dibasic acid anhydride, 0.1-2 parts of catalyst, 0.1-2 parts of antioxidant and 3-5 parts of sheet barrier. The corrosion resistance of 5% alkali solution was tested, which cannot meet the corrosion resistance requirements of high-concentration strong alkali. Summary of the invention

[0006] The purpose of the present invention is to provide a strong alkali resistant polyester resin and a preparation method thereof; a synthetic monomer containing a steric hindrance group is selected, and multifunctional alcohols are used for end-capping and a secondary vacuum process to effectively improve the steric hindrance effect and the curing crosslinking density, and reduce the residual carboxyl content in the polyester resin to less than 1 mgKOH / g, thereby reducing the reaction between the carboxyl group and the strong alkali.

[0007] Another object of the present invention is to provide a strong alkali resistant powder coating, the raw materials of which include the above-mentioned strong alkali resistant polyester resin, the coating has good leveling, mechanical properties, adhesion, and water boiling resistance. Under 30°C, after immersion in 50%wt NaOH for 96 hours, the coating has a gloss retention rate of more than 75%, without cracking, powdering, or falling off; under 60°C, after immersion in 50%wt NaOH for 22 hours, the coating has a gloss retention rate of more than 60%, without cracking, powdering, or falling off, and has excellent strong alkali resistance.

[0008] The specific technical solutions of the present invention are as follows:

[0009] A strong alkali-resistant polyester resin comprises the following raw materials in parts by weight:

[0010] 5.4-6.0 parts of polyol, 5.8-6.3 parts of polyacid, 0.05-0.35 parts of glycidyl ester, 0.008-0.012 parts of esterification catalyst, 0.1-0.3 parts of end-capping agent.

[0011] The polyol is a mixture of one or more of neopentyl glycol, 1,4-cyclohexanedimethanol and 2-butyl-2-ethyl-1,3-propanediol and 2,2,4-trimethyl-1,3-pentanediol, 2-methyl-1,3-propanediol, 1,6-hexanediol, trimethylolethane or trimethylolpropane, and at least one of trimethylolethane and trimethylolpropane is contained.

[0012] Preferably, the polyol is a mixture of neopentyl glycol, 1,4-cyclohexanedimethanol, 2-butyl-2-ethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-methyl-1,3-propanediol, 1,6-hexanediol, trimethylolethane, and trimethylolpropane in a mass ratio of 1.5-2.0:1.5-2.5:0.7-1.3:0-0.3:0-0.3:0-0.1:0-1.0:0-1.0, and at least one of trimethylolethane and trimethylolpropane is contained.

[0013] The polyacid is a mixture of terephthalic acid and one or more of isophthalic acid, 1,4-cyclohexanedicarboxylic acid, trimellitic anhydride and trimesic acid.

[0014] Preferably, in the polyacid, the mass ratio of terephthalic acid, isophthalic acid, 1,4-cyclohexanedicarboxylic acid, trimellitic anhydride and trimesic acid is 4.5-5.5:0-1.5:0-0.8:0-0.15:0-0.15.

[0015] The glycidyl ester is one or more of tertiary carbonic acid glycidyl ester or tertiary carbonic acid glycidyl ester and diglycidyl adipic acid, glycidyl methacrylate, and dimer acid diglycidyl ester. As a hydrophobic material, it can reduce the penetration of polar solvents or chemicals into the paint film and reduce the hydrolysis of ester bonds.

[0016] The esterification catalyst is monobutyltin oxide or stannous oxalate;

[0017] The end-capping agent is one or both of trimethylolethane and trimethylolpropane.

[0018] The alkali-resistant polyester resin has a hydroxyl value of 90-120 mgKOH / g, an acid value of 0-1 mgKOH / g, a viscosity of 2500-5000 mPa·s, and a glass transition temperature of 48-53°C.

[0019] The present invention provides a method for preparing a strong alkali-resistant polyester resin, comprising the following steps:

[0020] 1) Add the formulated amount of polyol into a reaction kettle, heat and melt, start stirring, then add the formulated amount of polyacid, esterification catalyst and glycidyl ester, raise the temperature to 230-240°C and maintain the reaction until the acid value reaches 5-10 mgKOH / g;

[0021] 2) cooling to 210-220° C., evacuating the mixture, and obtaining a polymer having an acid value of 0-2 mgKOH / g;

[0022] 3) Add a formulated amount of end-capping agent and maintain the reaction conditions for 30-60 minutes; evacuate the mixture again to obtain a strong alkali-resistant polyester resin.

[0023] In step 1), heating to 100-150° C. to melt;

[0024] The vacuuming in step 2) is carried out at -0.09 to -0.1 MPa for 2-3 hours.

[0025] The vacuuming reaction again in step 3) refers to vacuuming for 1-2h at -0.09 to -0.1MPa and 210-220°C.

[0026] In the synthesis process of the present invention, in the first step, alcohol and acid undergo an esterification reaction (reversible) to generate a low molecular weight polymer, and the introduction of a material containing a steric hindrance group (tert-butyl glycidyl carbonate and containing the same) can improve the effective spatial steric hindrance effect; in the second step, vacuum polycondensation is performed to increase the molecular weight, which is helpful to improve the impact, bending and other properties; in the third step, an end-capping agent is used for end-capping, followed by a secondary vacuum polycondensation, which further reduces the residual carboxyl groups at the ends of the molecular chains, reduces the possibility of reaction with a strong base, and improves the strong base resistance of the powder coating. Moreover, the monomers of the present invention contain larger groups and have better hydrophobicity. When introduced into the resin, they can reduce the penetration of polar solvents or chemicals into the paint film and reduce the hydrolysis of ester bonds, such as tert-butyl glycidyl carbonate and monomers with larger groups in the side chains (2-butyl-2-ethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, etc.); the residual carboxyl groups at the ends of the resin molecular weight react with alkali in a strong alkaline solution, which can easily cause corrosion of the coating. Secondary vacuum can reduce the residual carboxyl groups as much as possible; multifunctional alcohols can increase the degree of branching and the cross-linking density, thereby improving the corrosion resistance of the coating.

[0027] The alkali-resistant powder coating provided by the present invention comprises the above-mentioned alkali-resistant polyester resin as raw materials;

[0028] The alkali-resistant powder coating comprises the following raw materials in parts by weight: 35-50 parts of alkali-resistant polyester resin, 20-30 parts of isocyanate, 20-40 parts of pigment, 1.0-2.0 parts of leveling agent, 0.3-0.8 parts of benzoin, and 0.3-0.8 parts of wetting accelerator.

[0029] The isocyanate is selected from caprolactam blocked isocyanate, B1530;

[0030] The pigment is one or both of titanium dioxide and carbon black;

[0031] The leveling agent is GLP588;

[0032] The wetting promoter is BLC701B wetting promoter.

[0033] The preparation method of the strong alkali resistant powder coating is:

[0034] After fully premixing the raw materials in the formula, extrude them through a twin-screw extruder, and set the parameters as follows: zone I temperature 95-105°C, zone II temperature 105-120°C, zone III temperature 95-110°C, feeding speed frequency 25-35Hz, screw speed frequency 35-45Hz, and crush and grind the extruded flakes, and sieve them through a 200-mesh sieve to obtain the product.

[0035] The present invention selects monomers containing steric hindrance groups. In terms of alkali resistance, polyester resin contains a large number of ester bonds, and the ester bonds have poor alkali resistance. Effective steric hindrance can reduce the penetration of polar solvents and chemicals into the paint film and reduce the hydrolysis of ester bonds. The present invention uses multifunctional alcohols for end-capping and secondary vacuum process. The end-capping agent uses multifunctional alcohols, which can increase the branching degree, and the increase in curing cross-linking density is conducive to the improvement of strong alkali resistance; the secondary vacuum process can further reduce the residual carboxyl groups in the molecular chain and reduce the possibility of its reaction with strong alkali solution. The hydroxyl content of the polyester resin of the invention is 90-120 mgKOH / g, and the residual carboxyl content is reduced to less than 1 mgKOH / g. The prepared polyester resin is applied to powder coatings. Under the condition of 30°C, after being immersed in 50%wt NaOH for 96 hours, the gloss retention rate of the coating is greater than 75%, and there is no cracking, powdering or shedding phenomenon. Under the condition of 60°C, after being immersed in 50%wt NaOH for 22 hours, the gloss retention rate of the coating is greater than 60%, and there is no cracking, powdering or shedding phenomenon. The polyester resin has excellent strong alkali resistance. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0038] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0039] Example 1

[0040] A strong alkali-resistant polyester resin comprises the following raw materials in parts by weight: as shown in Table 1.

[0041] The preparation method of the strong alkali-resistant polyester resin in this embodiment 1 is specifically as follows:

[0042] According to Table 1, the formulated amount of polyol was put into the reactor, heated to 130°C to melt, stirred, and then the formulated amount of polyacid, esterification catalyst and tert-butyl glycidyl carbonate were added, and the temperature was raised to 235°C to maintain the reaction until the acid value was 5.9 mgKOH / g; the temperature was lowered to 215°C, and vacuumed for 2.5 hours at -0.1 MPa to obtain a polymer with an acid value of 1.5 mgKOH / g; the formulated amount of end-capping agent was added and maintained for 50 minutes; vacuumed for the second time. Vacuumed for 2 hours at -0.1 MPa and 215°C to obtain a strong alkali-resistant polyester resin with an acid value of 0.3 mgKOH / g, a viscosity of 3520 mPa·s, and a hydroxyl value of 99.6 mgKOH / g.

[0043] A strong alkali resistant powder coating, the raw materials of which include the strong alkali resistant polyester resin of the above-mentioned embodiment 1; the specific raw material components of the powder coating and their weight parts are shown in Table 2.

[0044] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 105° C., the temperature of zone II is 110° C., the temperature of zone III is 110° C., the feeding speed frequency is 30 Hz, and the screw speed frequency is 35 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain a strong alkali-resistant powder coating.

[0045] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0046] Example 2

[0047] A strong alkali-resistant polyester resin comprises the following raw materials in parts by weight: as shown in Table 1.

[0048] The preparation method of the strong alkali-resistant polyester resin in this embodiment 2 is specifically as follows:

[0049] According to Table 1, the polyol in the formula amount is put into the reaction kettle, heated to 120°C to melt, stirred, and then the polyacid, esterification catalyst and tert-butyl glycidyl carbonate in the formula amount are added, and the temperature is raised to 233°C to maintain the reaction until the acid value is 7.5 mgKOH / g; the temperature is lowered to 218°C, and vacuum is drawn at -0.1 MPa for 3 hours to obtain a polymer with an acid value of 1.6 mgKOH / g; the end-capping agent is added and maintained for 30 minutes; vacuum is drawn at -0.1 MPa and 212°C for 2 hours to obtain a strong alkali-resistant polyester resin with an acid value of 0.3 mgKOH / g, a viscosity of 3120 mPa·s, and a hydroxyl value of 98.3 mgKOH / g;

[0050] A strong alkali resistant powder coating, the raw materials of which include the strong alkali resistant polyester resin of the above-mentioned embodiment 2; the specific raw material components of the powder coating and their mass parts are shown in Table 2.

[0051] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 103° C., the temperature of zone II is 115° C., the temperature of zone III is 110° C., the feeding speed frequency is 35 Hz, and the screw speed frequency is 41 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain a strong alkali-resistant powder coating.

[0052] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0053] Example 3

[0054] A strong alkali-resistant polyester resin comprises the following raw materials in parts by weight: as shown in Table 1.

[0055] The preparation method of the strong alkali-resistant polyester resin in this embodiment 3 is specifically as follows:

[0056] According to Table 1, the polyol in the formula amount is put into the reaction kettle, heated to 110°C to melt, stirred, and then the polyacid, esterification catalyst and tert-butyl glycidyl carbonate in the formula amount are added, and the temperature is raised to 238°C to maintain the reaction until the acid value is 6.6 mgKOH / g; the temperature is lowered to 210°C, and vacuum is drawn at -0.1 MPa for 2 hours to obtain a polymer with an acid value of 1.0 mgKOH / g; the end-capping agent is added and maintained for 50 minutes; vacuum is drawn at -0.1 MPa and 220°C for 1.8 hours to obtain a strong alkali-resistant polyester resin with an acid value of 0.6 mgKOH / g, a viscosity of 2860 mPa·s, and a hydroxyl value of 110.1 mgKOH / g;

[0057] A strong alkali resistant powder coating, the raw materials of which include the strong alkali resistant polyester resin of the above-mentioned embodiment 3; the specific raw material components of the powder coating and their mass parts are shown in Table 2.

[0058] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 100° C., the temperature of zone II is 108° C., the temperature of zone III is 105° C., the feeding speed frequency is 33 Hz, and the screw speed frequency is 45 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain a strong alkali-resistant powder coating.

[0059] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0060] Example 4

[0061] A strong alkali-resistant polyester resin comprises the following raw materials in parts by weight: as shown in Table 1.

[0062] The preparation method of the strong alkali-resistant polyester resin in this embodiment 4 is specifically as follows:

[0063] According to Table 1, the polyol in the formula amount is put into the reaction kettle, heated to 125°C to melt, stirred, and then the polyacid, esterification catalyst and tert-butyl glycidyl carbonate in the formula amount are added, and the temperature is raised to 237°C to maintain the reaction until the acid value is 7.3 mgKOH / g; the temperature is lowered to 217°C, and vacuum is drawn at -0.1 MPa for 2.2 hours to obtain a polymer with an acid value of 1.7 mgKOH / g; the end-capping agent is added and maintained for 45 minutes; vacuum is drawn at -0.1 MPa and 210°C for 2 hours to obtain a strong alkali-resistant polyester resin with an acid value of 0.3 mgKOH / g, a viscosity of 3380 mPa·s, and a hydroxyl value of 96.5 mgKOH / g;

[0064] A strong alkali resistant powder coating, the raw materials of which include the strong alkali resistant polyester resin of the above-mentioned embodiment 4; the specific raw material components of the powder coating and their mass parts are shown in Table 2.

[0065] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 105° C., the temperature of zone II is 116° C., the temperature of zone III is 108° C., the feeding speed frequency is 30 Hz, and the screw speed frequency is 38 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain a strong alkali-resistant powder coating.

[0066] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0067] Example 5 (for comparison)

[0068] A polyester resin includes the following raw materials in parts by weight: as shown in Table 1.

[0069] The preparation method of the polyester resin in this embodiment 5 is specifically as follows:

[0070] According to Table 1, the polyol was put into a reaction kettle, heated to 120°C to melt, stirred, and then terephthalic acid and an esterification catalyst were added, and the temperature was raised to 235°C to maintain the reaction until the acid value was 6.0 mgKOH / g; the temperature was lowered to 215°C, and vacuum was drawn at -0.1 MPa for 1 hour to obtain a polyester resin with an acid value of 1.8 mgKOH / g, a viscosity of 3850 mPa·s, and a hydroxyl value of 100.2 mgKOH / g.

[0071] The above polyester resins are used in powder coatings.

[0072] The raw materials of the powder coating include the comparative polyester resin of Example 5 above; the specific raw material components of the powder coating and their weight parts are shown in Table 2.

[0073] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 98° C., the temperature of zone II is 116° C., the temperature of zone III is 105° C., the feeding speed frequency is 33 Hz, and the screw speed frequency is 44 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain the powder coating.

[0074] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0075] Example 6 (for comparison)

[0076] A polyester resin includes the following raw materials in parts by weight: as shown in Table 1.

[0077] The preparation method of the polyester resin in this embodiment 6 is specifically as follows:

[0078] According to Table 1, the polyol was added into a reaction kettle, heated to 122°C for melting, stirred, and then terephthalic acid, isophthalic acid and an esterification catalyst were added, and the temperature was raised to 233°C to maintain the reaction until the acid value was 6.2 mgKOH / g; the temperature was lowered to 211°C, and vacuum was drawn at -0.1 MPa for 1 hour to obtain a polymer with an acid value of 1.1 mgKOH / g; a capping agent was added and maintained for 37 minutes; vacuum was drawn at -0.1 MPa for 1.2 hours to obtain a polyester resin with an acid value of 0.8 mgKOH / g, a viscosity of 2730 mPa·s and a hydroxyl value of 90.8 mgKOH / g.

[0079] The above polyester resins are used in powder coatings.

[0080] The raw materials of the powder coating include the comparative polyester resin of Example 6 above; the specific raw material components of the powder coating and their weight parts are shown in Table 2.

[0081] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 93° C., the temperature of zone II is 111° C., the temperature of zone III is 104° C., the feeding speed frequency is 34 Hz, and the screw speed frequency is 44 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain the powder coating.

[0082] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0083] Example 7 (for comparison)

[0084] A polyester resin includes the following raw materials in parts by weight: as shown in Table 1.

[0085] The preparation method of the polyester resin in this embodiment 7 is specifically as follows:

[0086] According to Table 1, the polyol was put into a reaction kettle, heated to 111°C to melt, stirred, and then the polyacid, esterification catalyst and tert-butyl glycidyl carbonate were added, and the temperature was raised to 236°C to maintain the reaction until the acid value was 6.4 mgKOH / g; the temperature was lowered to 214°C, and vacuum was drawn at -0.1 MPa for 1.1 h to obtain a polyester resin with an acid value of 0.9 mgKOH / g, a viscosity of 3530 mPa·s, and a hydroxyl value of 91.5 mgKOH / g.

[0087] The above polyester resins are used in powder coatings.

[0088] The raw materials of the powder coating include the comparative polyester resin of Example 7 above; the specific raw material components of the powder coating and their weight parts are shown in Table 2.

[0089] The preparation method of the powder coating is as follows: raw materials are weighed according to the formula in Table 1, and the fully pre-mixed raw materials are extruded through a twin-screw extruder, and the parameters are set as follows: the temperature of zone I is 94° C., the temperature of zone II is 114° C., the temperature of zone III is 101° C., the feeding speed frequency is 39 Hz, and the screw speed frequency is 41 Hz. The extruded flakes are crushed, ground, and sieved through a 200-mesh screen to obtain the powder coating.

[0090] The prepared powder coating was electrostatically sprayed on an iron plate of a specific specification and cured at 200°C / 15min.

[0091] Table 1 Raw materials and weight parts of each example

[0092]

[0093] The underlined data in the table do not meet the requirements of the present invention.

[0094] The test standards are as follows: acid value test see standard GB / T 6743-2008; viscosity test see standard GB / T9751.1-2008; glass transition temperature (Tg) test, see standard GB / T 19466.2-2004.

[0095] Table 2 Powder coating raw materials mass parts and performance indicators

[0096]

[0097] The powder coating sample plates obtained in Examples 1-7 (double-sided spraying and corner kettle cover powder coating) were tested according to relevant test standards, wherein Example 5 is a conventional polyester resin for polyurethane powder coating, and Examples 6 and 7 are polyester resins synthesized using different raw materials and processes, which are used as reference and comparative resins for Examples 1-4 of the present invention, and were tested simultaneously according to the same test method, and the specific indicators are shown in Table 3. The test standards are as follows: Adhesion test sees standard GB / T 9286-1998; The gloss of the sample plate is directly measured by a gloss meter, see GB / T 9754; Impact resistance is tested by an impact meter of the state-owned Tianjin Instrument Testing Machine Factory, see GB / T 1732-93; Leveling performance is obtained by BYK leveling meter test; Bend test method GBT 6742-2007.

[0098] The method for testing the strong alkali resistance of powder coatings of the present invention is as follows: firstly, a sodium hydroxide solution with a mass fraction of 50% is prepared and poured into a container, half of the cured coating sample is immersed in the strong alkali solution, and then the container is sealed and placed in a water bath at a specific temperature. After being placed for a certain period of time, the sample is taken out, rinsed with distilled water, and the gloss retention rate and coating state of the coating are tested.

[0099] Table 3 Properties of powder coatings prepared from polyester resins in various embodiments

[0100]

[0101] It can be seen from the test results that the coating cured under the condition of 200℃ / 15min has good leveling, and there is no obvious change after the coating is boiled in water for 2 hours. In terms of mechanical properties, the resin of the present invention has excellent impact and bending properties, while the impact and bending properties of comparative examples 6 and 7 cannot meet the requirements. In the strong alkali resistance experiment, the powder coating of comparative example 5 has a light retention rate of 36% after immersion at 30℃ for 96h, and cracking and shedding phenomena occur in some areas of the coating. The light retention rates of the coatings of comparative examples 6 and 7 are 60.5% and 51.2% respectively, and cracking phenomena occur in some areas of the coating, while the light retention rate of the resin of the present invention is greater than 75%, and the coating surface is intact without cracking, powdering, or shedding phenomena; after immersion at 60℃ for 22h, the coating of comparative example 5 loses gloss seriously, and large-area powdering and shedding phenomena occur. The light retention rates of comparative examples 6 and 7 are reduced to less than 10%, and cracking and shedding phenomena occur in some areas of the coating, while the light retention rate of the resin coating of the present invention is greater than 60%, without cracking, powdering, or shedding phenomena, and has excellent strong alkali resistance.

[0102] In addition, after being corroded by 5% alkali solution at room temperature for 500 hours, there was no change in the samples of Examples 1 to 4, and the light retention rate was still greater than 80% after 45 days of the experiment.

Claims

1. A strong alkali resistant polyester resin, characterized in that: The alkali-resistant polyester resin comprises the following raw materials in parts by weight: 5.4-6.0 parts of polyol, 5.8-6.3 parts of polyacid, 0.05-0.35 parts of glycidyl ester, 0.008-0.012 parts of esterification catalyst, 0.1-0.3 parts of end-capping agent; The polyol is a mixture of one or more of neopentyl glycol, 1,4-cyclohexanedimethanol and 2-butyl-2-ethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-methyl-1,3-propanediol, 1,6-hexanediol, trimethylolethane or trimethylolpropane, and at least one of trimethylolethane and trimethylolpropane is contained; The polyacid is a mixture of terephthalic acid and one or more of isophthalic acid, 1,4-cyclohexanedicarboxylic acid, trimellitic anhydride, and trimesic acid; in the polyacid, the mass ratio of terephthalic acid, isophthalic acid, 1,4-cyclohexanedicarboxylic acid, trimellitic anhydride, and trimesic acid is 4.5-5.5:0-1.5:0-0.8:0-0.15:0-0.15; the end-capping agent is one or two of trimethylolethane and trimethylolpropane; The glycidyl ester is tert-butyl glycidyl carbonate or a mixture of tert-butyl glycidyl carbonate and diglycidyl adipate, glycidyl methacrylate, and diglycidyl dimer acid; The alkali-resistant polyester resin has a hydroxyl value of 90-120 mgKOH / g, an acid value of 0-1 mgKOH / g, a viscosity of 2500-5000 mPa·s, and a glass transition temperature of 48-53°C.

2. The alkali-resistant polyester resin according to claim 1, characterized in that: The polyol is a mixture of neopentyl glycol, 1,4-cyclohexanedimethanol, 2-butyl-2-ethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-methyl-1,3-propanediol, 1,6-hexanediol, trimethylolethane and trimethylolpropane in a mass ratio of 1.5-2.0:1.5-2.5:0.7-1.3:0-0.3:0-0.3:0-0.1:0-1.0:0-1.0, and at least one of trimethylolethane and trimethylolpropane is contained.

3. A method for preparing the alkali-resistant polyester resin according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: 1) Add the formulated amount of polyol into a reactor, heat and melt, start stirring, then add the formulated amount of polyacid, esterification catalyst and glycidyl ester, raise the temperature to 230-240℃ and maintain the reaction until the acid value reaches 5-10 mgKOH / g; 2) Cooling to 210-220°C, evacuating, and obtaining a polymer with an acid value of 0-2 mgKOH / g; 3) Add a formulated amount of end-capping agent and maintain the reaction conditions for 30-60 minutes; evacuate the mixture again to obtain a strong alkali-resistant polyester resin.

4. The preparation method according to claim 3, characterized in that: The vacuuming in step 2) is performed at -0.1 MPa for 2-3 hours.

5. The preparation method according to claim 3 or 4, characterized in that: The vacuuming reaction again in step 3) refers to vacuuming for 1-2 hours at -0.09 to -0.1 MPa and 210-220°C.

6. A strong alkali resistant powder coating, characterized in that: The alkali-resistant powder coating comprises the alkali-resistant polyester resin according to claim 1 or 2.