A preparation method of thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite

By introducing thiol-functionalized graphene oxide, the mechanical properties and combustion properties of BAMO-AMMO-ETPE are improved, the problem of poor mechanical properties is solved, and the stress and combustion heat are increased.

CN115850945BActive Publication Date: 2024-10-15XIAN MODERN CHEM RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211596644.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-15
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

The mechanical properties of BAMO-AMMO-ETPE are poor. Existing improvement methods mainly change its structure and do not use additives to improve performance.

Method used

By introducing thiol functionalized graphene oxide and changing its addition amount, the mechanical properties of BAMO-AMMO-ETPE are improved, its decomposition is promoted and the combustion heat is increased. The specific method includes pre-treating BAMO-AMMO-ETPE, ultrasonic dispersion of thiol-functionalized graphene oxide and BAMO-AMMO-ETPE, mixing evenly and leaving to form.

Benefits of technology

The stress and strain of BAMO-AMMO-ETPE are increased, the amount of thermal decomposition residue is reduced, the combustion performance is enhanced, the combustion heat is increased by 100.16J/g~477.27J/g, and the preparation method is simple and the cost is low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115850945B_ABST
    Figure CN115850945B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a thiol-functionalized graphene oxide / 3,3-bis-azidomethyl-3-methyl-oxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared by the method can improve the mechanical properties of the original BAMO-AMMO-ETPE, increase the stress by 0.91MPa to 3.28MPa, increase the strain by 1.23 to 2.85, promote the decomposition of BAMO-AMMO-ETPE, reduce the amount of residue after thermal decomposition of BAMO-AMMO-ETPE by 3.19% to 13.78%, enhance the combustion performance of BAMO-AMMO-ETPE, increase the combustion heat of BAMO-AMMO-ETPE by 100.16J / g to 477.27J / g, and the preparation method is easy and has low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of energetic materials, and in particular relates to a method for preparing a thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxytetracyclyl and 3-azidomethyl-3-methyloxytetracyclyl energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. Background Art

[0002] Energetic thermoplastic elastomers (ETPEs) as solid propellant binders can give propellants advantages such as high energy, insensitivity, low characteristic signals and recyclability. Azide energetic thermoplastic elastomers have attracted widespread attention due to their high heat release, no need for oxygen consumption during decomposition, and good compatibility with nitramine explosives. Poly (3,3'-bisazidomethylbutylene oxide) (BAMO) has a high energy level, while 3-azidomethyl-3'-methylbutylene oxide (AMMO) has excellent mechanical properties and low-temperature mechanical properties. Their copolymers are considered to be the preferred binders for the next generation of propellants with the most promising application prospects. BAMO-AMMO-ETPE has a high glass transition temperature and density, but its mechanical properties are poor.

[0003] At present, the main method to improve the mechanical properties of BAMO-AMMO-ETPE is to introduce different groups into its preparation. Gan Xiaoxian et al. prepared BAMO-AMMO-ETPE with a number average molecular weight of about 25,000 using Sanderson's synthesis method in the article "Synthesis and Properties of BAMO / AMMO-based ETPE" (Journal of Explosives and Propellants, 2008, 31(2): 81-85). The synthesized copolymer has the characteristics of being fusible and soluble, and the room temperature tensile strength and elongation are about 5MPa and 400%. Chi Zhang et al. used carbon nanotubes (CNT-OH) instead of traditional additive trimethylolethane (TME) to prepare CNT-OH / BAMO-AMMO-ETPE, in which the tensile strength reached 10.4MPa and the thermal decomposition temperature was 236°C. The methods reported so far all change the structure of BAMO-AMMO-ETPE through reaction to improve its performance, and do not improve the performance of BAMO-AMMO-ETPE with a certain structure through additives. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the defects and shortcomings existing in the background technology and provide a method for preparing a thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxytetracyclyl and 3-azidomethyl-3-methyloxytetracyclyl energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite.

[0005] In order to solve the above technical problems, the overall idea of ​​the present invention is: by introducing thiol-functionalized graphene oxide into BAMO-AMMO-ETPE to prepare a composite, without changing the synthesis method of BAMO-AMMO-ETPE, by changing the amount of thiol-functionalized graphene oxide added, the mechanical properties of BAMO-AMMO-ETPE are improved, the decomposition of BAMO-AMMO-ETPE is promoted, and the combustion heat of BAMO-AMMO-ETPE is increased.

[0006] In order to achieve the above technical tasks, the present invention adopts the following technical solutions:

[0007] Compared with the prior art, the present invention has the following beneficial technical effects:

[0008] A method for preparing a thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite comprises the following steps:

[0009] Step 1: pre-treating BAMO-AMMO-ETPE;

[0010] Step 2: mixing 3-mercaptopropyltriethoxysilane-modified graphene oxide with acetone, and then performing ultrasonic dispersion to obtain a thiol-functionalized graphene oxide dispersion;

[0011] Step 3: Mix the pretreated BAMO-AMMO-ETPE with acetone, filter out the insoluble matter, and obtain BAMO-AMMO-ETPE clear solution;

[0012] Step 4: Pour the thiol-functionalized graphene oxide dispersion obtained in step 2 into the BAMO-AMMO-ETPE clear solution obtained in step 3, raise the mixed solution to the reflux temperature range during the BAMO-AMMO-ETPE pretreatment, stir evenly, then perform ultrasonic dispersion, and let stand to form, to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite

[0013] Furthermore, the method for pretreating BAMO-AMMO-ETPE in step 1 comprises:

[0014] Step 1-1: reflux and precipitate BAMO-AMMO-ETPE in acetone;

[0015] Step 1-2: Filter out the white flocculent precipitate to obtain the pretreated BAMO-AMMO-ETPE.

[0016] Preferably, in the step 2, the dosage ratio of 3-mercaptopropyltriethoxysilane-modified graphene oxide to acetone is: 5 mg to 80 mg: 12 g to 220 g. After the 3-mercaptopropyltriethoxysilane-modified graphene oxide and acetone are mixed, ultrasonic dispersion is carried out in a temperature range of 20 to 35° C. for 1 to 2 hours.

[0017] Preferably, the ratio of the pretreated BAMO-AMMO-ETPE to acetone is: 2g-10g:40g-126g; stirring at a temperature range of 20-35°C for 1-2h, filtering out insoluble matter, and obtaining BAMO-AMMO-ETPE clear solution.

[0018] In the step 4, the 3-mercaptopropyltriethoxysilane modified graphene oxide dispersion obtained in step 2 is poured into the BAMO-AMMO-ETPE clear solution obtained in step 3, the mixed solution is raised to the reflux temperature range of 55-60° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6-8 hours, and ultrasonically dispersed for 20-40 minutes in the temperature range of 20-35° C., and allowed to stand for molding.

[0019] The prepared thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite can improve the mechanical properties of the original BAMO-AMMO-ETPE, increase the stress by 0.91MPa to 3.28MPa, increase the strain by 1.23 to 2.85, promote the decomposition of BAMO-AMMO-ETPE, reduce the amount of residue after thermal decomposition of BAMO-AMMO-ETPE by 3.19% to 13.78%, enhance the combustion performance of BAMO-AMMO-ETPE, increase the combustion heat of BAMO-AMMO-ETPE by 100.16J / g to 477.27J / g, and the preparation method is easy and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a strain-stress diagram of the raw material BAMO-AMMO-ETPE prepared according to an embodiment of the present invention.

[0021] Figure 2 This is a TG diagram of thermal decomposition of the raw material BAMO-AMMO-ETPE prepared in an embodiment of the present invention.

[0022] Figure 3 It is a strain-stress diagram of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1 of the present invention.

[0023] Figure 4 This is a TG diagram of thermal decomposition of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1 of the present invention.

[0024] Figure 5 This is a SEM image of the raw material BAMO-AMMO-ETPE composite prepared in Example 1 of the present invention.

[0025] Figure 6 This is a SEM image of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1 of the present invention.

[0026] Figure 7 This is an infrared image of the raw material BAMO-AMMO-ETPE prepared in an embodiment of the present invention.

[0027] Figure 8 This is an infrared image of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1 of the present invention.

[0028] The details of the present invention are explained below in conjunction with specific implementation methods. DETAILED DESCRIPTION

[0029] In the reaction raw materials of the present invention, the structure of thiol-functionalized graphene oxide is as follows:

[0030]

[0031] The raw material preparation process and method refer to the relevant content of the team's prior application CN 112062784 B.

[0032] The raw materials involved in the present invention include BAMO-AMMO-ETPE prepared according to the method disclosed in the literature "Synthesis and Properties of BAMO / AMMO-based ETPE", Journal of Explosives and Propellants, 31(2): 81-85. The relative molecular mass of BAMO-AMMO-ETPE is 25000, the stress is 3.26MPa, the strain is 6.47, the residue amount in TG test is 16.7%, and the heat of combustion is 24287.13J / g. Figure 1 and 2 They are the strain-stress diagram and TG thermal decomposition diagram of the raw material BAMO-AMMO-ETPE involved in the preparation.

[0033] Example 1

[0034] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0035] 30 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 90 g of acetone and ultrasonically dispersed at 25° C. for 1.5 h. 4.0 g of the pretreated BAMO-AMMO-ETPE was added to 96 g of acetone and stirred at 25° C. for 1.5 h. The insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 55° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6 hours, and ultrasonically dispersed for 20 to 40 min in the temperature range of 20 to 35° C., and then allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the related thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite was 6.54MPa, which was 3.28MPa higher than that of BAMO-AMMO-ETPE, the strain was 9.32, which was 2.85 higher, the residue was 2.92%, which was 13.78% lower than that of BAMO-AMMO-ETPE, and the heat of combustion was 24764.4J / g, which was 477.27J / g higher than that of BAMO-AMMO-ETPE. Figure 3 and Figure 4 They are respectively the strain stress diagram and thermal decomposition TG diagram of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1 of the present invention.

[0036] Structural analysis

[0037] 1. Scanning electron microscopy (SEM) analysis

[0038] The surface morphology of BAMO-AMMO-ETPE and its composite was studied using a scanning electron microscope. Pure BAMO-AMMO-ETPE is relatively smooth, but when thiol-functionalized graphene oxide is added, the BAMO-AMMO-ETPE composite becomes relatively rough, and flakes of thiol-functionalized graphene oxide can be seen, with BAMO-AMMO-ETPE coated on top. Figure 5 This is the SEM image of the raw material BAMO-AMMO-ETPE prepared in Example 1. Figure 6 This is a SEM image of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1.

[0039] 2. Infrared analysis

[0040] The infrared spectrum of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is similar to that of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite because the amount of thiol-functionalized graphene oxide added is small and its characteristic peaks, such as functional groups such as hydroxyl and alkoxy, are also present in BAMO-AMMO-ETPE. Figure 7 This is the infrared image of the prepared raw material BAMO-AMMO-ETPE. Figure 8 This is an infrared image of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite prepared in Example 1.

[0041] Example 2

[0042] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0043] 60 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 138 g of acetone and ultrasonically dispersed at 35° C. for 2 h. 10.0 g of pretreated BAMO-AMMO-ETPE was added to 218 g of acetone, stirred at 30° C. for 1.5 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 57° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6.3 hours, and ultrasonically dispersed for 20 to 40 min in the temperature range of 20 to 35° C., and then allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 6.08 MPa, the strain is 9.04, the residue amount is 3.78%, and the heat of combustion is 24700.8 J / g.

[0044] Example 3

[0045] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0046] 55 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 112 g of acetone and ultrasonically dispersed at 33° C. for 2 h. 4.8 g of pretreated BAMO-AMMO-ETPE was added to 102 g of acetone and stirred at 32° C. for 2 h. The insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 58° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 7.1 hours, and ultrasonically dispersed for 20 to 40 min in the temperature range of 20 to 35° C., and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 4.79 MPa, the strain is 8.14, the residue amount is 10.74%, and the heat of combustion is 24459.67 J / g.

[0047] Example 4

[0048] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0049] 43 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 92 g of acetone and ultrasonically dispersed at 25° C. for 2 h. 5.3 g of pretreated BAMO-AMMO-ETPE was added to 214 g of acetone and stirred at 27° C. for 2 h. The insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 57° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6.4 hours, and ultrasonically dispersed for 20 to 40 min in the temperature range of 20 to 35° C., and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 4.73 MPa, the strain is 8.25, the residue amount is 8.97%, and the heat of combustion is 24672.47 J / g.

[0050] Example 5

[0051] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0052] 47 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 106 g of acetone and ultrasonically dispersed at 28° C. for 2 h. 5.3 g of pretreated BAMO-AMMO-ETPE was added to 164 g of acetone, stirred at 27° C. for 1.4 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 55° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 7.2 hours, and ultrasonically dispersed for 20 to 40 min in the temperature range of 20 to 35° C., and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 5.85 MPa, the strain is 8.02, the residue amount is 11.79%, and the heat of combustion is 24588.63 J / g.

[0053] Example 6

[0054] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0055] 37 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 96 g of acetone and ultrasonically dispersed at 28° C. for 2 h. 3.3 g of pretreated BAMO-AMMO-ETPE was added to 62 g of acetone, stirred at 22° C. for 1.8 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 56° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6 hours, and ultrasonically dispersed for 20 to 40 min in the temperature range of 20 to 35° C., and then allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 5.98 MPa, the strain is 8.42, the residue amount is 8.69%, and the heat of combustion is 24485.63 J / g.

[0056] Example 7

[0057] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0058] 32 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 86 g of acetone and ultrasonically dispersed at 30° C. for 1 h. 5.3 g of pretreated BAMO-AMMO-ETPE was added to 103 g of acetone, stirred at 28° C. for 1.8 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 59° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6.8 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 6.09 MPa, the strain is 8.19, the residue amount is 13.06%, and the heat of combustion is 24625.87 J / g.

[0059] Example 8

[0060] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0061] 28 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 75 g of acetone and ultrasonically dispersed at 33° C. for 2 h. 6.3 g of pretreated BAMO-AMMO-ETPE was added to 210 g of acetone, stirred at 27° C. for 1.2 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE clear solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 59° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 7.8 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 6.08 MPa, the strain is 4.93, the residue amount is 3.68%, and the heat of combustion is 24399.15 J / g.

[0062] Example 9

[0063] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0064] 25 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 61 g of acetone and ultrasonically dispersed at 33° C. for 1.6 h. 3.3 g of pretreated BAMO-AMMO-ETPE was added to 63 g of acetone, stirred at 29° C. for 1.2 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE clear solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 60° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 7.1 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 5.29 MPa, the strain is 7.98, the residue amount is 6.76%, and the heat of combustion is 24687.96 J / g.

[0065] Example 10

[0066] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0067] 19 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 51 g of acetone and ultrasonically dispersed at 33° C. for 2 h. 2.8 g of pretreated BAMO-AMMO-ETPE was added to 53 g of acetone, stirred at 30° C. for 1.6 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 57° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain 5.7 g of the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) complex. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 5.86 MPa, the strain is 7.91, the residue amount is 11.85%, and the heat of combustion is 24716.85 J / g.

[0068] Embodiment 11

[0069] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0070] 10 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 71 g of acetone and ultrasonically dispersed at 36° C. for 2 h. 2.0 g of pretreated BAMO-AMMO-ETPE was added to 31 g of acetone, stirred at 28° C. for 1.6 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 58° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 8 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 5.18 MPa, the strain is 8.76, the residue amount is 5.64%, and the heat of combustion is 24559.85 J / g.

[0071] Example 12

[0072] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0073] 6 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 32 g of acetone and ultrasonically dispersed at 36° C. for 1.5 h. 6.0 g of pretreated BAMO-AMMO-ETPE was added to 151 g of acetone, stirred at 28° C. for 1.6 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE clear solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 59° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6.9 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite has a stress of 4.87 MPa, a strain of 8.63, a residue amount of 9.76%, and a combustion heat of 24689.12 J / g.

[0074] Example 13

[0075] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0076] 5 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 18 g of acetone and ultrasonically dispersed at 25° C. for 1.5 h. 2.0 g of pretreated BAMO-AMMO-ETPE was added to 51 g of acetone and stirred at 26° C. for 1.9 h. The insoluble matter was filtered out to obtain BAMO-AMMO-ETPE solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 60° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6.9 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The stress of the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite is 5.71 MPa, the strain is 8.99, the residue amount is 3.67%, and the heat of combustion is 24613.74 J / g.

[0077] Embodiment 14

[0078] BAMO-AMMO-ETPE was refluxed and precipitated in acetone; the white flocculent precipitate was filtered out to obtain the pretreated BAMO-AMMO-ETPE.

[0079] 10 mg of 3-mercaptopropyltriethoxysilane modified graphene oxide was added to 18 g of acetone and ultrasonically dispersed at 25° C. for 1.5 h. 8.0 g of pretreated BAMO-AMMO-ETPE was added to 126 g of acetone, stirred at 35° C. for 2 h, and the insoluble matter was filtered out to obtain BAMO-AMMO-ETPE clear solution. The ultrasonically dispersed thiol-functionalized graphene oxide dispersion was poured into the BAMO-AMMO-ETPE solution, and the mixed solution was raised to the reflux temperature range of 60° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 8 hours, and ultrasonically dispersed in the temperature range of 20 to 35° C. for 20 to 40 min, and allowed to stand for molding to obtain the corresponding thiol-functionalized graphene oxide / 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer (BAMO-AMMO-ETPE) composite. The thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite has a stress of 5.41 MPa, a strain of 8.22, a residue amount of 10.97%, and a combustion heat of 24597.37 J / g.

Claims

1. A method for preparing a thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite, characterized in that: The steps include: Step 1: pretreating 3,3-bis-azidomethyloxybutylene and 3-azidomethyl-3-methyloxybutylene energetic thermoplastic elastomer BAMO-AMMO-ETPE; Step 2: mixing 3-mercaptopropyltriethoxysilane-modified graphene oxide with acetone, and then performing ultrasonic dispersion to obtain a thiol-functionalized graphene oxide dispersion; Step 3: Mix the pretreated BAMO-AMMO-ETPE with acetone, filter out the insoluble matter, and obtain a BAMO-AMMO-ETPE clear solution; Step 4: Pour the thiol-functionalized graphene oxide dispersion obtained in step 2 into the BAMO-AMMO-ETPE clear solution obtained in step 3, raise the mixed solution to the reflux temperature range during the BAMO-AMMO-ETPE pretreatment, stir evenly, then perform ultrasonic dispersion, and let stand to form, to obtain the corresponding thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite.

2. The method for preparing the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite according to claim 1, characterized in that: The method for pretreating BAMO-AMMO-ETPE in step 1 comprises: Step 1-1: reflux and precipitate BAMO-AMMO-ETPE in acetone; Step 1-2: Filter out the white flocculent precipitate to obtain the pretreated BAMO-AMMO-ETPE.

3. The method for preparing the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite according to claim 2, characterized in that: In the step 2, the dosage ratio of 3-mercaptopropyltriethoxysilane-modified graphene oxide to acetone is: 5 mg to 80 mg: 12 g to 220 g. After the 3-mercaptopropyltriethoxysilane-modified graphene oxide and acetone are mixed, ultrasonic dispersion is carried out in a temperature range of 20 to 35° C. for 1 to 2 hours.

4. The method for preparing the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite according to claim 2, characterized in that: The ratio of the pretreated BAMO-AMMO-ETPE to acetone is: 2g-10g: 40g-126g; stirring for 1-2h at a temperature range of 20-35°C, filtering the insoluble matter, and obtaining a BAMO-AMMO-ETPE clear solution.

5. The method for preparing the thiol-functionalized graphene oxide / BAMO-AMMO-ETPE composite according to claim 2, characterized in that: In the step 4, the 3-mercaptopropyltriethoxysilane modified graphene oxide dispersion obtained in step 2 is poured into the BAMO-AMMO-ETPE clear solution obtained in step 3, the mixed solution is raised to the reflux temperature range of 55-60° C. during the BAMO-AMMO-ETPE pretreatment, and then uniformly stirred for 6-8 hours, and ultrasonically dispersed for 20-40 minutes in the temperature range of 20-35° C., and then allowed to stand for molding.