Precursor composition for preparing polymer electrolyte, and polymer electrolyte and secondary battery prepared using the same

By using a precursor composition with a specific composition to prepare a polymer electrolyte, the problems of low ionic conductivity and insufficient safety in lithium secondary batteries are solved, and the high-temperature stability and flame retardancy are improved, thus improving the overall performance of the battery.

CN115868057BActive Publication Date: 2026-11-10LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180051008.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2021-12-03
Publication Date
2026-11-10
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

In existing lithium secondary batteries, polymer electrolytes suffer from low ionic conductivity, deteriorated output characteristics, and insufficient high-temperature stability. Furthermore, liquid electrolytes are flammable, posing safety hazards.

Method used

A polymer electrolyte is prepared by polymerization reaction using a precursor composition consisting of lithium salt, non-aqueous organic solvent, polymerization initiator, oligomer represented by Formula 1 and compound represented by Formula 2 in a specific ratio, thereby improving lithium ion transport and flame retardancy.

Benefits of technology

It improves the oxidation potential and flame retardancy of the polymer electrolyte, enhances the safety and high-temperature output characteristics of the lithium secondary battery, and ensures the stability and safety of battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention relates to a precursor composition for preparing a polymer electrolyte, and a polymer electrolyte and a secondary battery prepared by using the same. The precursor composition for preparing a polymer electrolyte of the present invention comprises a lithium salt, a non-aqueous organic solvent, a polymerization initiator, an oligomer represented by Formula 1, and a compound represented by Formula 2, wherein the oligomer represented by Formula 1 and the compound represented by Formula 2 are included in a weight ratio of 1:0.01 to 1:4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Cross-reference to related applications

[0002] This application claims priority to Korean Patent Application No. 10-2020-0182200, filed on December 23, 2020, and Korean Patent Application No. 10-2021-0170874, filed on December 2, 2021, the disclosures of which are incorporated herein by reference. Technical Field

[0004] This invention relates to a precursor composition for preparing a polymer electrolyte, and to a polymer electrolyte and a secondary battery prepared using the precursor composition. Background Technology

[0005] Recently, attention has been growing towards energy storage technology. In particular, as the application of energy storage technology has expanded to mobile phones, cameras, laptops, and even electric vehicles, research and efforts have been made to develop energy storage technologies.

[0006] Electrochemical devices have received the most attention in the field of energy storage technology, and among these devices, rechargeable secondary batteries have generated interest. In particular, lithium-ion batteries, developed in the early 1990s, have become a focal point due to their high operating voltage and extremely high energy density.

[0007] In lithium secondary batteries, liquid electrolytes in which salts are dissolved in non-aqueous solvents are mainly used. However, liquid electrolytes are prone to low stability and battery performance degradation because they decompose more easily during continuous charging and discharging, and they are also prone to combustion due to the increase in ambient temperature and the temperature of the battery itself.

[0008] To address this issue, efforts have recently been made to develop secondary batteries that use polymer electrolytes with a lower risk of combustion.

[0009] However, due to the excellent electrochemical safety of polymer electrolytes, it is advantageous that they not only maintain a constant battery thickness but also enable the fabrication of thin-film batteries, as the inherent adhesive force of the gel phase results in excellent adhesion between the electrode and the electrolyte. However, in contrast, when separation occurs due to the different phases of the non-aqueous organic solvent in the electrolyte and the polymer matrix, the lithium ions are not uniformly positioned in the polymer electrolyte, leading to another problem of reduced ionic conductivity and deteriorated output characteristics.

[0010] Therefore, there is a need to develop polymer electrolytes that can improve the performance of secondary batteries by improving lithium-ion transport properties while ensuring high-temperature stability. Summary of the Invention

[0011] Technical issues

[0012] One aspect of the present invention provides a precursor composition for preparing polymer electrolytes, wherein the oxidation potential and flame retardancy are increased and the viscosity is reduced.

[0013] Another aspect of the present invention provides a polymer electrolyte prepared by using the precursor composition for preparing a polymer electrolyte.

[0014] Another aspect of the present invention provides a lithium secondary battery with improved capacity characteristics by including the polymer electrolyte.

[0015] Technical solution

[0016] According to one aspect of the present invention, a precursor composition for preparing a polymer electrolyte is provided, the precursor composition comprising:

[0017] Lithium salts, non-aqueous organic solvents, polymerization initiators,

[0018] Oligomers represented by Equation 1, and

[0019] The compound represented by formula 2,

[0020] The oligomer represented by Formula 1 and the compound represented by Formula 2 comprise, in a weight ratio of 1:0.01 to 1:4:

[0021] [Formula 1]

[0022]

[0023] In Equation 1,

[0024] R, R1, and R2 are each independently an alkyl group having 1 to 5 carbon atoms.

[0025] A and A' are each independently a unit containing one or more (meth)acrylate groups.

[0026] B is a unit containing at least one amide group, and

[0027] n, m, and k are the number of repeating units.

[0028] Where n is an integer from 1 to 10,000,

[0029] m is an integer from 1 to 1,000, and

[0030] k is an integer from 1 to 100.

[0031] [Equation 2]

[0032]

[0033] In Formula 2, R3 is -CR5=CH2 (where R5 is hydrogen or an alkyl group having 1 to 4 carbon atoms) or -R6-CF3 (where R6 is an alkyl group having 1 to 20 carbon atoms and substituted with at least one fluorine molecule).

[0034] R4 is an alkyl or alkyl group having 1 to 20 carbon atoms and being unsubstituted or substituted with at least one fluorine atom, where p is an integer of 0 or 1, and

[0035] When R3 is -R6-CF3, p is 0, and R4 is an alkyl group having 1 to 20 carbon atoms that is not fluorinated.

[0036] According to another aspect of the present invention, a polymer electrolyte prepared by using the polymer composition for preparing a polymer electrolyte is provided.

[0037] According to another aspect of the present invention, a lithium secondary battery comprising the polymer electrolyte is provided.

[0038] Beneficial effects

[0039] Since the oligomer represented by Formula 1 (which is included in the precursor composition for preparing polymer electrolytes of the present invention) can reduce the surface tension of the precursor composition for preparing polymer electrolytes by including polycarbonate groups that have excellent reactivity with non-aqueous organic solvents as main chain repeating units, it can improve the moisturizing properties of the precursor composition for preparing polymer electrolytes.

[0040] Furthermore, since the ester compound represented by Formula 2 (which is included in the precursor composition for preparing polymer electrolytes of the present invention) can increase the degree of aggregation and crystallinity in the polymer matrix by including a substituent containing at least one fluorine, it can reduce the viscosity of the precursor composition for preparing polymer electrolytes and at the same time improve the flame retardancy and oxidation potential of the electrolyte.

[0041] Therefore, if the precursor composition for preparing a polymer electrolyte of the present invention, which includes oligomers represented by Formula 1 and compounds represented by Formula 2 together in a specific combination ratio, is used, a polymer electrolyte with improved oxidation potential and flame retardancy and suppression of gas generation can be prepared by the synergistic effect of these compounds, and a lithium secondary battery with improved overall performance (such as safety and high-temperature output characteristics) can be achieved by using the polymer electrolyte. Detailed Implementation

[0042] The invention will now be described in more detail to allow for a clearer understanding of it.

[0043] It will be understood that the terms and terminology used in the specification and claims should not be interpreted as having the meanings defined in common dictionaries. It will be further understood that, based on the principle that the inventor may appropriately define the meanings of terms or terms to best illustrate the invention, these terms and terms should be interpreted as having meanings consistent with their meanings in the relevant field and in the context of the technical concept of the invention.

[0044] The terminology used in this specification is for describing exemplary embodiments only and is not intended to limit the invention. Singular terms may include plural forms unless the opposite is mentioned.

[0045] It will be further understood that the terms “comprising,” “including,” or “having” in this specification indicate the presence of the stated features, quantities, steps, elements, or combinations thereof, without excluding the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.

[0046] Unless otherwise stated in this invention, the expression "*" indicates the same or different atoms or parts connected between the ends of a formula.

[0047] [Precursor compositions for the preparation of polymer electrolytes]

[0048] According to one embodiment, the present invention provides a precursor composition for preparing a polymer electrolyte, the precursor composition comprising:

[0049] Lithium salts, non-aqueous organic solvents, polymerization initiators,

[0050] Oligomers represented by Equation 1, and

[0051] The compound represented by formula 2,

[0052] The oligomer represented by Formula 1 and the compound represented by Formula 2 are comprised in a weight ratio of 1:0.01 to 1:4.

[0053] [Formula 1]

[0054]

[0055] In Equation 1,

[0056] R, R1, and R2 are each independently an alkyl group having 1 to 5 carbon atoms.

[0057] A and A' are each independently a unit containing one or more (meth)acrylate groups.

[0058] B is a unit containing at least one amide group, and

[0059] n, m, and k are the number of repeating units.

[0060] Where n is an integer from 1 to 10,000,

[0061] m is an integer from 1 to 1,000, and

[0062] k is an integer from 1 to 100.

[0063] The amide group refers to the group formed by... The group indicated.

[0064] [Equation 2]

[0065]

[0066] In Equation 2,

[0067] R3 is -CR5=CH2 (where R5 is hydrogen or an alkyl group having 1 to 4 carbon atoms) or -R6-CF3 (where R6 is an alkyl group having 1 to 20 carbon atoms and substituted with at least one fluorine molecule).

[0068] R4 is an alkyl or alkyl group having 1 to 20 carbon atoms and being unsubstituted or substituted with at least one fluorine atom, where p is an integer of 0 or 1, and

[0069] When R3 is -R6-CF3, p is 0, and R4 is an alkyl group having 1 to 20 carbon atoms that is not fluorinated.

[0070] (1) Lithium salts

[0071] Any lithium salt commonly used in electrolytes for lithium secondary batteries can be used as the lithium salt without limitation, and, for example, the lithium salt may include Li. + As a cation, and may include at least one of the following groups as an anion: F - Cl - ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - B 10 Cl 10 - AlCl4 - AlO2 - PF6 - CF3SO3 - CH3CO2- CF3CO2 - AsF6 - SbF6 - CH3SO3 - (CF3CF2SO2)2N - (CF3SO2)2N - (FSO2)2N - BF2C2O4 - BC4O8 - PF4C2O4 - PF2C4O8 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO - (CF3SO2)2CH - CF3(CF2)7SO3 - and SCN - .

[0072] Specifically, lithium salts may include a single material or a mixture of two or more materials selected from the group consisting of: LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 The following materials can be used without restriction: LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2 (Lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2 (Lithium bis(pentafluoroethanesulfonyl)imide, LiBETI), and LiN(SO2CF3)2 (Lithium bis(trifluoromethanesulfonyl)imide, LiTFSI).

[0073] The lithium salt can be appropriately varied within the normal usable range, but can have a concentration of 0.8M to 4.0M (e.g., 1.0M to 3.0M) to obtain the best effect of forming a film that prevents corrosion of the electrode surface.

[0074] If the concentration of lithium salt is less than 0.8 M, the effect of improving the cycling characteristics during low-temperature output and high-temperature storage is minimal due to the reduced mobility of lithium ions. Furthermore, if the concentration of lithium salt is greater than 4.0 M, the impregnability of the precursor composition used to prepare the polymer electrolyte may be reduced due to the excessive increase in viscosity.

[0075] (2) Non-aqueous organic solvents

[0076] Various non-aqueous organic solvents commonly used in lithium electrolytes can be used as non-aqueous organic solvents without limitation. For example, non-aqueous organic solvents may include organic solvents based on cyclic carbonates, organic solvents based on linear carbonates, or mixed non-aqueous organic solvents of the above.

[0077] Organic solvents based on cyclic carbonates are highly viscous non-aqueous organic solvents that can readily dissociate lithium salts in electrolytes due to their high dielectric constant. Specific examples of organic solvents based on cyclic carbonates may be at least one non-aqueous organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butenyl carbonate, 2,3-butenyl carbonate, 1,2-pentenyl carbonate, 2,3-pentenyl carbonate, and vinylene carbonate, and among them, organic solvents based on cyclic carbonates may include at least one of ethylene carbonate and propylene carbonate (PC).

[0078] Furthermore, linear carbonate-based organic solvents are non-aqueous organic solvents with low viscosity and low dielectric constant. Typical examples of linear carbonate-based organic solvents may be at least one non-aqueous organic solvent selected from the group consisting of: dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and linear carbonate-based organic solvents may particularly include ethyl methyl carbonate (EMC).

[0079] Organic solvents based on cyclic carbonates and organic solvents based on linear carbonates can be mixed and used as non-aqueous organic solvents. In this case, the organic solvents based on cyclic carbonates and organic solvents based on linear carbonates can be used in a volume ratio of 10:90 to 80:20, for example, 50:50 to 70:30.

[0080] In addition, in order to prepare an electrolyte with high ionic conductivity, the non-aqueous organic solvent may further include organic solvents based on straight-chain esters and / or organic solvents based on cyclic carbonates and / or organic solvents based on linear carbonates, which have lower melting points and higher stability at high temperatures.

[0081] As a representative example, organic solvents based on straight-chain esters may include at least one non-aqueous organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and may particularly include ethyl propionate and / or propyl propionate.

[0082] In addition, organic solvents based on cyclic esters may include at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.

[0083] In the precursor compositions of the present invention for preparing polymer electrolytes, the remainder may be entirely non-aqueous organic solvents, except for lithium salts, oligomers represented by Formula 1 and compounds represented by Formula 2, unless otherwise stated.

[0084] (3) Polymerization initiator

[0085] Next, the polymerization initiator will be described.

[0086] The polymerization initiator is used to initiate the polymerization reaction of oligomers included in the precursor composition for preparing polymer electrolytes of the present invention.

[0087] For example, organic peroxides or hydroperoxides (such as benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, t-butylperoxy-2-ethyl-hexanoate, cumyl hydroperoxide, and hydrogen peroxide) and azo compounds (such as 2,2'-azobis(2-cyanobutane), 2,2'-azobis(methylbutyronitrile), 2,2'-azobis(isobutyronitrile) (AIBN, 2,2'-Azobisdimethyl-Valeronitrile)) can be used as polymerization initiators, but polymerization initiators are not limited to these.

[0088] The polymerization initiator is a material that can decompose to form free radicals at room temperature (25°C to 30°C) or, as a non-limiting example, at 30°C to 100°C, wherein the oligomers can be polymerized by the free radicals to react with acrylate-based compounds to form a polymer electrolyte.

[0089] Based on 100 parts by weight of the oligomer represented by Formula 1, 0.01 to 5 parts by weight, preferably 0.05 to 5 parts by weight, and more preferably 0.1 to 5 parts by weight, of a polymerization initiator can be used. Using a polymerization initiator within the above range prevents gelation during the injection of the precursor composition for preparing the polymer electrolyte into the battery and minimizes the amount of unreacted polymerization initiator that could adversely affect battery performance. In other words, when the polymerization initiator is included within the above range, gelation can be appropriately achieved.

[0090] (4) Oligomers represented by Equation 1

[0091] Next, the oligomers represented by Equation 1 will be described.

[0092] Generally, polymer electrolytes suffer from disadvantages such as poorer safety and mechanical properties compared to solid polymer electrolytes, and lower conductivity compared to liquid electrolytes. In particular, polymer electrolytes using oligomers as the sole additive are unsuitable for high-capacity, large-scale batteries due to difficulties in controlling physical properties and uniformly distributing the polymer within the battery. Therefore, recent research has focused on improving the mechanical properties or conductivity of polymer electrolytes by using a polymer matrix formed from the polymerization of oligomers. However, during the preparation of polymer electrolytes, non-aqueous organic solvents are typically used as precursor compositions. Since the phase of the non-aqueous organic solvent is liquid while the three-dimensional polymer matrix formed by combining oligomers is solid, phase separation may occur due to the density difference between the polymer matrix and the non-aqueous organic solvent. If this separation occurs in the battery, the conductivity of the secondary battery decreases due to the uneven distribution of lithium ions within the electrolyte.

[0093] Therefore, in order to solve these problems, oligomers are used in this invention, which include units having functional groups with properties similar to those of non-aqueous organic solvents.

[0094] In other words, the oligomers of the present invention can improve the reactivity between the polymer matrix formed from the oligomers and the non-aqueous organic solvents by including polycarbonate groups with properties similar to those of non-aqueous organic solvents as repeating units in the main chain. Therefore, since lithium ions can be uniformly located in the electrolyte, the conductivity can be improved. Furthermore, since the polycarbonate groups constituting the oligomer main chain have a high affinity for metal oxides, the adhesion between the polymer electrolyte of the present invention prepared from the oligomers represented by Formula 1 and the electrode using metal oxides is improved, thereby further improving the cycle performance and stability of the battery.

[0095] The oligomers of the present invention capable of achieving this effect may include compounds represented by the following formula 1.

[0096] [Formula 1]

[0097]

[0098] In Equation 1,

[0099] R, R1, and R2 are each independently an alkyl group having 1 to 5 carbon atoms.

[0100] A and A' are each independently a unit containing one or more (meth)acrylate groups.

[0101] B is a unit containing at least one amide group, and

[0102] n, m, and k are the number of repeating units.

[0103] Where n is an integer from 1 to 10,000,

[0104] m is an integer from 1 to 1,000, and

[0105] k is an integer from 1 to 100.

[0106] The amide group refers to the group formed by... The group indicated.

[0107] In Formula 1, A and A' may each independently include at least one (meth)acrylate group from the units represented by Formulas A-1 to A-6 below. In particular, to improve the mechanical properties of the polymer electrolyte, it is more desirable for units A and A' to include at least one unit selected from the units represented by Formulas A-3 to A-6 below, which are more readily crosslinked.

[0108] [Formula A-1]

[0109]

[0110] [Formula A-2]

[0111]

[0112] [Formula A-3]

[0113]

[0114] [Formula A-4]

[0115]

[0116] [Formula A-5]

[0117]

[0118] [Formula A-6]

[0119]

[0120] Furthermore, in the oligomers represented by Formula 1 of the present invention, unit B, which includes at least one amide group, is a functional group that controls the ion transport properties of the polymer electrolyte and imparts the ability to control mechanical properties and adhesive forces, wherein unit B may include units represented by the following formula B-1.

[0121] [Formula B-1]

[0122]

[0123] In equation B-1,

[0124] R' is an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted or substituted cycloalkyl group having 3 to 10 carbon atoms, an unsubstituted or substituted bicycloalkyl group having 6 to 20 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 20 carbon atoms.

[0125] In particular, R' may include at least one of the units selected from those represented by the following formulas R'-1 to R'-6.

[0126] [Equation R'-1]

[0127]

[0128] [Equation R'-2]

[0129]

[0130] [Formula R'-3]

[0131]

[0132] [Equation R'-4]

[0133]

[0134] [Formula R'-5]

[0135]

[0136] [Formula R'-6]

[0137]

[0138] Furthermore, in Equation 1, n is preferably an integer from 5 to 5,000, for example, an integer from 5 to 1,000. When n is within the aforementioned range, a viscosity level suitable for smooth wetting can be ensured, and electrochemical stability can be improved.

[0139] In particular, the oligomers represented by Formula 1 of the present invention may include oligomers represented by Formula 1A.

[0140] [Formula 1A]

[0141]

[0142] In Equation 1A,

[0143] R, R1, and R2 are each independently an alkyl group having 1 to 5 carbon atoms.

[0144] R' is an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted or substituted cycloalkyl group having 3 to 10 carbon atoms, an unsubstituted or substituted bicycloalkyl group having 6 to 20 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 20 carbon atoms.

[0145] A and A' are each independently a unit containing one or more (meth)acrylate groups, and

[0146] n, m, and k are the number of repeating units.

[0147] Where n is an integer from 1 to 10,000,

[0148] m is an integer from 1 to 1,000, and

[0149] k is an integer from 1 to 100.

[0150] More specifically, the oligomer represented by Formula 1 can be a compound represented by Formula 1A-1.

[0151] [Formula 1A-1]

[0152]

[0153] In Equation 1A-1,

[0154] n1, m1, and k1 are the number of repeating units.

[0155] Where n1 is an integer from 1 to 10,000.

[0156] m1 is an integer from 1 to 1,000, and

[0157] k1 is an integer from 1 to 100.

[0158] a and a' are each an independent integer of 1 or 2, and

[0159] b and b' are each an independent integer from 1 to 3.

[0160] More specifically, the oligomer represented by Formula 1 can be a compound represented by the following Formula 1A-2.

[0161] [Equation 1A-2]

[0162]

[0163] In Equation 1A-2,

[0164] n2, m2, and k2 are the number of repeating units.

[0165] Where n2 is an integer from 1 to 10,000.

[0166] m2 is an integer from 1 to 1,000, and

[0167] k2 is an integer from 1 to 100.

[0168] As described above, the oligomers of the present invention improve the reactivity with non-aqueous organic solvents by including polycarbonate groups as main chain repeating units, thereby increasing the ionic conductivity of the electrolyte. Furthermore, since the polycarbonate groups have a high affinity for metal oxides, improving the adhesion between the electrode and the electrolyte using metal oxides, battery stability can be improved. However, since the polycarbonate groups have relatively low reactivity with graphite-based compounds, the adhesion to the electrode using graphite as the electrode material may be reduced to some extent. Therefore, the adhesion between the electrolyte and the electrode comprising the oligomer can be adjusted to a certain level or higher by including amide groups (urethane groups) that have high reactivity with graphite in the oligomer.

[0169] Based on the total weight of the precursor composition used to prepare the polymer electrolyte, the oligomer represented by Formula 1 may be included in an amount from 0.1 wt% to 30 wt%, particularly from 0.1 wt% to 25 wt%, and preferably from 0.1 wt% to 15 wt%. Where the amount of oligomer meets the above range, viscosity, strength, and ionic conductivity exceeding predetermined levels for application in the battery can be ensured.

[0170] Furthermore, according to embodiments of the present invention, the weight-average molecular weight (Mw) of the oligomer represented by Formula 1 can be controlled by the number of repeating units and can be in the range of about 1,000 g / mol to about 1,500,000 g / mol, particularly in the range of 2,000 g / mol to about 1,200,000 g / mol, and even more particularly in the range of 2,000 g / mol to 1,000,000 g / mol. When the weight-average molecular weight of the oligomer is within the above-mentioned range, the mechanical strength of the battery comprising the oligomer can be effectively improved. In this case, the weight-average molecular weight in this specification can represent the equivalent value of standard polystyrene measured by gel permeation chromatography (GPC), and unless otherwise stated, the molecular weight can represent the weight-average molecular weight. For example, in the present invention, the weight-average molecular weight is measured using the Agilent Technologies 1200 series, in which case an Agilent Technologies PL mixed B column can be used, and tetrahydrofuran (THF) can be used as a solvent.

[0171] (5) Compounds represented by Equation 2

[0172] In order to reduce the viscosity of the precursor composition for preparing polymer electrolytes by increasing the degree of aggregation and crystallinity in the polymer matrix, and at the same time improve the flame retardancy and oxidation potential of the electrolyte, in addition to the oligomer represented by Formula 1, the precursor composition for preparing polymer electrolytes according to the present invention may further include a compound as an additive.

[0173] The compound is a monomer with low electrical resistance, wherein it is substituted with at least one fluorine, and the compound can be represented by the following formula 2.

[0174] [Equation 2]

[0175]

[0176] In Equation 2,

[0177] R3 is -CR5=CH2 (where R5 is hydrogen or an alkyl group having 1 to 3 carbon atoms) or -R6-CF3 (where R6 is an alkyl group having 1 to 20 carbon atoms and substituted with at least one fluorine molecule).

[0178] R4 is an alkyl or alkyl group having 1 to 20 carbon atoms and being unsubstituted or substituted with at least one fluorine atom, where p is an integer of 0 or 1, and

[0179] When R3 is -R6-CF3, p is 0, and R4 is an alkyl group having 1 to 20 carbon atoms that is not fluorinated.

[0180] Specifically, R3 is -CR5=CH2 (wherein R5 is hydrogen or an alkyl group having 1 to 3 carbon atoms) or -R6-CF3 (wherein R6 is an alkyl group having 1 to 10 carbon atoms and substituted with at least one fluorine), R4 is an alkyl or alkyl group having 1 to 10 carbon atoms and not substituted with or substituted with at least one fluorine, p is an integer of 0 or 1, and when R3 is -R6-CF3, p is 0, and R4 can be an alkyl group having 1 to 10 carbon atoms and not substituted with fluorine.

[0181] More specifically, the compound represented by Formula 2 may include at least one compound selected from the group consisting of compounds represented by Formulas 2-1 to 2-8.

[0182] [Equation 2-1]

[0183]

[0184] [Equation 2-2]

[0185]

[0186] [Equation 2-3]

[0187]

[0188] [Equation 2-4]

[0189]

[0190] [Equation 2-5]

[0191]

[0192] [Equation 2-6]

[0193]

[0194] [Equation 2-7]

[0195]

[0196] [Equation 2-8]

[0197]

[0198] Based on the total weight of the precursor composition used to prepare the polymer electrolyte, it may include 0.01 wt% to 45 wt%, particularly 0.01 wt% to 30 wt%, and especially 0.1 wt% to 30 wt% of the compound represented by Formula 2. When the amount of the compound represented by Formula 2 included is within the above range, when the oligomers form a three-dimensional polymer network, the compound represented by Formula 2 can further reduce the viscosity of the precursor composition used to prepare the polymer electrolyte by increasing the degree of aggregation and crystallinity in the polymer. Furthermore, the compound represented by Formula 2 can improve the flame retardancy and oxidation potential of the precursor composition through fluorine, thereby preventing a decrease in battery safety. Additionally, since the free radical reaction rate during the polymer reaction can be increased, a polymer electrolyte with better mechanical properties can be formed.

[0199] The oligomers represented by Formula 1 and the compounds represented by Formula 2 may be included in a weight ratio of 1:0.01 to 1:4.

[0200] If the oligomers represented by Formula 1 and the compounds represented by Formula 2 are included within the aforementioned range, the flame retardancy and oxidation potential of the precursor compositions used to prepare the polymer electrolyte can be improved. The charging and discharging of the battery can be stabilized by causing lithium ions to dissociate in the electrolyte to a level higher than a predetermined level, and viscosity can be maintained at a level at which the moisturizing properties in the battery can be consistently preserved. In particular, if the weight ratio of the compound represented by Formula 2 to the oligomer represented by Formula 1 is 4 or less, the overall performance of the battery, such as battery operating performance, including resistance and output characteristics, can be improved by reducing electrochemical interference reactions. Furthermore, if the weight ratio of the compound represented by Formula 2 is 0.01 or greater, the flame retardancy and oxidation potential of the polymer electrolyte can be effectively improved.

[0201] As described above, when the weight ratio of the compound represented by Formula 2 to the oligomer represented by Formula 1 satisfies the above numerical range, the viscosity of the precursor composition of the present invention for preparing polymer electrolytes can be improved, and polymer electrolytes that ensure excellent ionic conductivity and flame retardancy can be prepared.

[0202] Specifically, it may include oligomers represented by Formula 1 and compounds represented by Formula 2 in weight ratios of 1:0.1 to 1:4, such as 1:1 to 1:4.

[0203] Compounds containing two or more acrylate groups as end groups, such as those represented by Formula 3, have a higher viscosity than solvents based on carbonates, which are common electrolyte solvents. Therefore, when a compound represented by Formula 3 is included as a component of the precursor composition for preparing the polymer electrolyte of the present invention, instead of a compound represented by Formula 1, the increased viscosity of the precursor composition for preparing the polymer electrolyte reduces lithium-ion mobility, and the electrochemical performance of the polymer electrolyte deteriorates due to reduced impregnation, thus relatively deteriorating battery performance.

[0204] [Formula 3]

[0205]

[0206] (6) Other additives

[0207] Furthermore, if necessary, in addition to the compounds represented by Formula 1, the precursor compositions of the present invention for preparing polymer electrolytes may further include additional additives to prevent negative electrode collapse due to the decomposition of non-aqueous organic solvents under high power conditions, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and the effect of suppressing battery expansion at high temperatures.

[0208] Examples of other additives may be at least one selected from the group consisting of: unsubstituted or substituted halogen-based carbonate compounds, sulfonyl lactone-based compounds, sulfate-based compounds, phosphate-based or phosphite-based compounds, borate-based compounds, nitrile compounds, phenyl compounds, amino compounds, silane-based compounds, and lithium-based compounds.

[0209] Halogen-unsubstituted or substituted carbonate-based compounds may include, for example, vinylene carbonate (VC), vinyl ethylene carbonate, or fluoroethylene carbonate (FEC).

[0210] The sulfonyl-based compound can be, for example, at least one compound selected from the group consisting of: 1,3-propanesulfonyl lactone (PS), 1,4-butanesulfonyl lactone, ethanesulfonyl lactone, 1,3-propenesulfonyl lactone (PRS), 1,4-butenesulfonyl lactone, and 1-methyl-1,3-propenesulfonyl lactone.

[0211] Sulfuric acid-based compounds can be, for example, ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS).

[0212] The phosphate-based or phosphite-based compound may be, for example, at least one compound selected from the group consisting of: lithium difluoro(bis(oxalato)phosphate), lithium difluorophosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.

[0213] Borate-based compounds can be tetraphenol borates, lithium difluorooxalate borate (LiODFB), or lithium bis(oxalate borate) (LiB(C2O4)2; LiBOB).

[0214] The nitrile compound may be, for example, at least one compound selected from the group consisting of: succinate, adiponitrile, acetonitrile, propionitrile, butyronitrile, valerate, octanonitrile, n-heptanonitrile, cyclopentaneformitrile, cyclohexaneformitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.

[0215] The phenyl compound can be a fluorobenzene, the amino compound can be triethanolamine or ethylenediamine, and the silyl compound can be tetraethylenesilane.

[0216] The lithium-based compound is a compound that is different from the lithium salt included in the precursor composition used to prepare the polymer electrolyte, wherein the lithium-based compound may include LiPO2F2 or LiBF4.

[0217] In the case of other additives such as vinylene carbonate, vinyl ethylene carbonate, or succinate, a more robust solid electrolyte interphase (SEI) can be formed on the surface of the negative electrode during the initial activation process of the secondary battery.

[0218] In the case of LiBF4, the high-temperature stability of the secondary battery can be improved by suppressing the generation of gases that may be generated during high-temperature storage due to electrolyte decomposition.

[0219] Two or more compounds may be mixed and used as other additives, and based on the total weight of the precursor composition used to prepare the polymer electrolyte, other additives may be included in amounts ranging from 0.01 wt% to 50 wt%, particularly from 0.05 wt% to 10 wt%, and especially from 0.1 wt% to 5 wt%. If the amount of additional additives is less than 0.01 wt%, the effect on improving the battery's low-temperature output, high-temperature storage characteristics, and high-temperature life characteristics is minimal, while if the amount of additional additives is greater than 50 wt%, excessive side reactions may occur during battery charging and discharging due to the excessive amount of additives. In particular, when excessive amounts of additives are added to form the SEI, these additives may not decompose sufficiently at high temperatures, resulting in the formation of unreacted materials in the electrolyte at room temperature, or they may exist in the form of precipitates. Consequently, side reactions that degrade the life or resistivity characteristics of the secondary battery may occur.

[0220] [Polymer electrolyte]

[0221] The polymer electrolyte according to the present invention will now be described.

[0222] The polymer electrolytes of the present invention can be prepared by using the precursor compositions of the present invention for preparing polymer electrolytes.

[0223] Conventional polymer electrolytes suffer from the following problems: lower conductivity than liquid electrolytes, and relatively poorer stability (such as flame retardancy) and mechanical properties compared to solid polymer electrolytes. However, the polymer electrolyte according to the invention achieves improved conductivity and mechanical properties by comprising a polymer network formed using oligomers represented by Formula 1, which includes: units comprising polycarbonate groups as repeating units in the main chain; unit B comprising amide groups; and units A and A' comprising (meth)acrylate groups. In particular, since the oligomers represented by Formula 1 include polycarbonate groups as repeating units, which have properties similar to non-aqueous organic solvents, separation caused by phase difference between the non-aqueous organic solvent and the oligomer can be suppressed, and accordingly, lithium ions are uniformly distributed in the electrolyte, thus improving the conductivity of the polymer electrolyte.

[0224] Furthermore, the polymer electrolyte according to the present invention can improve oxidation potential and flame retardancy by using compounds of Formula 2 containing fluorine as additives. In particular, since the compounds represented by Formula 2 can enhance the polymerization reaction of oligomers by promoting the free radical reaction of polymers, the mechanical properties of the polymer electrolyte can be improved, and the side reactions of the electrolyte can be suppressed by increasing the electrode protection effect of the polymer. Therefore, the effect of improving the life characteristics and durability of secondary batteries can be achieved.

[0225] Therefore, in the case of polymer electrolytes, if the output characteristics and oxidation resistance are improved by increasing the lithium-ion mobility, a lithium secondary battery with improved overall performance (such as oxidation safety and high-temperature output characteristics) can be realized.

[0226] The polymer electrolyte according to the invention can be formed by polymerization of a precursor composition for preparing the polymer electrolyte using conventional methods known in the art. In particular, the polymer electrolyte can be formed by in-situ polymerization of the precursor composition for preparing the polymer electrolyte in a secondary battery (described later).

[0227] More specifically, as will be described below, the polymer electrolyte can be prepared by the following steps: (a) inserting an electrode assembly consisting of a positive electrode, a negative electrode and a separator disposed between the positive and negative electrodes into a battery housing; and (b) adding a precursor composition according to the invention for preparing a polymer electrolyte into the battery housing and performing polymerization to form a polymer electrolyte.

[0228] In-situ polymerization in lithium secondary batteries can be carried out using electron beams, gamma rays, and room temperature / high temperature aging treatments. According to embodiments of the invention, in-situ polymerization in lithium secondary batteries can also be carried out via thermal polymerization. In this case, the required polymerization time can range from about 2 minutes to about 12 hours, and the thermal polymerization temperature can range from 30°C to 100°C.

[0229] More specifically, after the polymerization initiator, quantitative amounts of oligomers represented by Formula 1 and compounds represented by Formula 2 are added to a non-aqueous solvent in which lithium salts are dissolved and mixed. The mixture is then injected into the battery cell, and the in-situ polymerization reaction in the lithium secondary battery is carried out by sealing the injection port of the battery cell and heating the battery cell at 40°C to 80°C for 1 to 20 hours.

[0230] As another method, an electrode assembly is prepared by winding or stacking the electrodes and / or separators on which the polymer electrolyte is formed after coating a precursor composition for preparing a polymer electrolyte onto one surface of an electrode and a separator and curing it with heat or UV (gelling). A lithium secondary battery can be prepared by inserting the electrode assembly into a battery housing and re-injecting it with a conventional liquid electrolyte.

[0231] [Lithium-ion rechargeable battery]

[0232] Next, the lithium secondary battery according to the present invention will be described.

[0233] A lithium secondary battery according to another embodiment of the present invention includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a polymer electrolyte, and in this case, the polymer electrolyte is the polymer electrolyte according to the present invention. Since the polymer electrolyte has been described above, the description thereof will be omitted and other components will be described below.

[0234] (1) Positive Electrode

[0235] The positive electrode according to the present invention may include a positive electrode active material layer containing a positive electrode active material, and if necessary, the positive electrode active material layer may further include a conductive agent and / or a binder.

[0236] The positive electrode active material is a compound capable of reversibly intercalating and deintercalating lithium, wherein the positive electrode active material may particularly include a lithium composite metal oxide including lithium and at least one metal selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), iron (Fe), and aluminum (Al), and may include a high-nickel (Ni) lithium composite metal oxide in which the Ni content is 0.55 or higher.

[0237] Typical examples of the lithium composite metal oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.7 Mn 0.20 Co 0.10 )O2, Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, Li[Ni 0.8 Co 0.15 Al 0.05 O2, Li[Ni 0.86 Mn 0.07 Co 0.05 Al 0.02 O2 or Li(Ni 0.9 Mn 0.05 Co 0.05 )O2.

[0238] In addition, in addition to the above lithium composite metal oxides, the positive electrode active material may further include lithium manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), lithium cobalt-based oxides (e.g., LiCoO2, etc.), lithium nickel-based oxides (e.g., LiNiO2, etc.), lithium nickel manganese-based oxides (e.g., LiNi 1-Y Mn Y O2 (where 0<Y<1), LiMn 2-Z Ni z O4 (where 0<Z<2)), lithium nickel cobalt-based oxides (e.g., LiNi1-Y1 Co Y1 O2 (where 0<Y1<1)), lithium manganese cobalt-based oxides (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0<Y2<1), LiMn 2-Z1 Co z1 O4 (where 0<Z1<2)), lithium nickel manganese cobalt-based oxides (e.g., Li(Ni p Co q Mn r1 )O2 (where 0<p<1, 0<q<1, 0<r1<1 and p+q+r1=1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0<p1<2, 0<q1<2, 0<r2<2 and p1+q1+r2=2) or lithium nickel cobalt transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3 M S2 )O2) (where M is selected from the group consisting of aluminum (Al), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), tantalum (Ta), magnesium (Mg), and molybdenum (Mo), and p2, q2, r3 and s2 are the atomic fractions of each independent element, where 0<p2<1, 0<q2<1, 0<r3<1, 0<S2<1 and p2+q2+r3+S2=1), if necessary.

[0239] Based on the total weight of the positive electrode active material layer, the positive electrode active material may be included in an amount of 80 wt% to 98 wt%, for example 85 wt% to 98 wt%. When the positive electrode active material is included in an amount within the above range, excellent capacity characteristics can be exhibited.

[0240] Next, the conductive agent is used to provide electrical conductivity to the electrode, and any conductive agent may be used without particular limitation as long as it has suitable electronic conductivity and does not cause adverse chemical changes in the battery.

[0241] As specific examples of the conductive agent, conductive materials such as: carbon powders such as carbon black, acetylene black (or Denka black), Ketjen black, channel black, furnace black, lamp black or thermal black; graphite powders such as natural graphite, artificial graphite, or graphite having a well-grown crystal structure; conductive fibers such as carbon fibers or metal fibers; conductive powders such as fluorocarbon powder, aluminum powder and nickel powder; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; or polyphenylene derivatives may be used.

[0242] Based on the total weight of the positive electrode active material layer, it may include 0.1% to 10% by weight, for example, 0.1% to 5% by weight of a conductive agent.

[0243] Next, the adhesive improves the adhesion between the positive electrode active material particles and the adhesion between the positive electrode active material and the current collector.

[0244] Specific examples of adhesives may be: fluoropolymer-based adhesives, including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based adhesives, including styrene-butadiene rubber (SBR), nitrile rubber, or styrene-isoprene rubber; cellulose-based adhesives, including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, or regenerated cellulose; polyol-based adhesives, including polyvinyl alcohol; polyolefin-based adhesives, including polyethylene or polypropylene; polyimide-based adhesives; polyester-based adhesives; and silane-based adhesives.

[0245] Based on the total weight of the positive electrode active material layer, it may include 0.1% to 15% by weight, for example, 0.1% to 10% by weight of an amount of adhesive.

[0246] The positive electrode of the present invention described above can be prepared by methods known in the art for preparing positive electrodes. For example, the positive electrode can be prepared by coating a positive electrode slurry onto a positive electrode current collector, wherein the positive electrode slurry is prepared by dissolving or dispersing a positive electrode active material, a binder, and / or a conductive agent in a solvent, drying, and then rolling; or the positive electrode can be prepared by pouring the positive electrode slurry onto a separate support and then laminating a film layer separated from the support onto the positive electrode current collector.

[0247] The positive electrode current collector is not particularly limited, as long as it is conductive and will not cause adverse chemical changes in the battery. For example, it can be made of stainless steel, aluminum, nickel, titanium, combusted carbon, or aluminum or stainless steel with a surface treated with carbon, nickel, titanium, silver, or the like. Furthermore, the positive electrode current collector typically has a thickness from 3 μm to 500 μm, and minute irregularities can be formed on the surface of the current collector to improve the adhesion of the positive electrode material. For example, positive electrode current collectors of various shapes can be used, such as films, sheets, foils, meshes, porous bodies, foams, nonwovens, and similar shapes.

[0248] The solvent can be any solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and any one of them or a mixture of two or more of them may be used. If the cathode material mixture can be adjusted to have appropriate viscosity taking into account the coating thickness, manufacturing yield, and processability of the cathode material mixture, the amount of solvent used may be sufficient, and the amount of solvent is not particularly limited.

[0249] (2) Negative electrode

[0250] Next, the negative electrode will be described.

[0251] Lithium metal electrodes, such as lithium, copper, or nickel electrodes, can be used as the negative electrode according to the present invention.

[0252] Alternatively, a negative electrode including various negative electrode active materials used in the art can be used as the negative electrode of the present invention, such as carbon-based negative electrode active materials, silicon-based negative electrode active materials, or mixtures thereof.

[0253] The negative electrode active material may include carbon-based negative electrode active materials, and various carbon-based negative electrode active materials used in the art can be used as carbon-based negative electrode active materials, such as graphite-based materials (such as natural graphite, artificial graphite, and Kish graphite), pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, high-temperature sintered carbon (such as petroleum orcoal tar pitch-derived cokes), soft carbon, and hard carbon. The shape of the carbon-based negative electrode active material is not particularly limited, and materials of various shapes can be used, such as irregular shapes, planar shapes, sheet-like, spherical, or fibrous forms.

[0254] Preferably, the carbon-based negative electrode active material may include at least one of natural graphite and artificial graphite. More preferably, the carbon-based negative electrode active material may include both natural graphite and artificial graphite. When natural graphite and artificial graphite are used together, the adhesion to the current collector can be increased to inhibit the shedding of the active material.

[0255] According to another embodiment, the negative active material may include a carbon-based negative active material and a silicon-based negative active material.

[0256] Specific examples of the carbon-based negative active material are the same as those described above.

[0257] The silicon-based negative active material may, for example, include at least one selected from the group consisting of metal silicon (Si), silicon oxide (SiO x , where 0<x<2), silicon carbide (SiC), and Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si). Element Y may be selected from the group consisting of Mg, calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), Ti, zirconium (Zr), hafnium (Hf), rutherfordium (Rf), V, niobium (Nb), Ta, (dubnium; Db), Cr, Mo, tungsten (W), (seaborgium; Sg), technetium (Tc), rhenium (Re), (bohrium; Bh), Fe, lead (Pb), ruthenium (Ru), osmium (Os), (hassium; Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), Al, gallium (Ga), tin (Sn), indium (In), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), and combinations thereof.

[0258] Since the silicon-based negative active material has higher capacity characteristics than the carbon-based negative active material, better capacity characteristics can be obtained when the silicon-based negative active material is further included.

[0259] In terms of weight ratio, the mixing ratio of the silicon-based negative active material : the carbon-based negative active material may be in the range of 3:97 to 99:1, for example, 5:95 to 15:85. In the case where the mixing ratio of the silicon-based negative active material and the carbon-based negative active material satisfies the above range, since the volume expansion of the silicon-based negative active material is suppressed while the capacity characteristics are improved, excellent cycle performance can be ensured.

[0260] The negative active material may be included in an amount of 80 wt% to 99 wt%, based on the total weight of the negative active material layer. In the case where the amount of the negative active material satisfies the above range, excellent capacity characteristics and electrochemical properties can be obtained.

[0261] The negative active material layer may further include a conductive agent and / or a binder, if necessary.

[0262] A conductive agent is a component used to further improve the conductivity of the negative electrode active material. Any conductive agent can be used without particular limitation, as long as it is conductive and does not cause adverse chemical changes in the battery. This conductive agent can be the same as or different from the conductive agent used during the preparation of the positive electrode. Specifically, conductive materials can be used as conductive agents, such as: carbon powder, such as carbon black, acetylene black (or Denka black), Ketjen black, channel black, furnace black, lamp black, or thermally cracked carbon black; graphite powder, such as natural graphite, artificial graphite, or graphite with a well-grown crystal structure; conductive fibers, such as carbon fibers or metal fibers; conductive powders, such as fluorocarbon powder, aluminum powder, and nickel powder; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polystyrene derivatives.

[0263] Based on the total weight of the negative electrode active material layer, a conductive agent of 10% by weight or less, such as 5% by weight or less, can be added.

[0264] The adhesive is a component that facilitates the bonding of conductive agents, active materials, and current collectors, and may be the same as or different from the adhesive used during the fabrication of the positive electrode. Specifically, the adhesive may include: fluoropolymer-based adhesives, including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based adhesives, including styrene-butadiene rubber (SBR), nitrile rubber, or styrene-isoprene rubber; cellulose-based adhesives, including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, or regenerated cellulose; polyol-based adhesives, including polyvinyl alcohol; polyolefin-based adhesives, including polyethylene or polypropylene; polyimide-based adhesives; polyester-based adhesives; and silane-based adhesives.

[0265] Based on the total weight of the negative electrode active material layer, an amount of binder can be added from 0.1% to 20% by weight.

[0266] The negative electrode can be prepared using methods known in the art. For example, the negative electrode can be prepared by coating a negative electrode slurry onto a negative electrode current collector, the slurry being prepared by dissolving or dispersing a negative electrode active material, along with optional binders and conductive agents, in a solvent, followed by rolling and drying; or the negative electrode can be prepared by pouring the negative electrode slurry onto a separate support and then laminating a film layer separated from the support onto the negative electrode current collector.

[0267] The negative electrode current collector is not particularly limited, as long as it has high conductivity and will not cause adverse chemical changes in the battery. For example, it can be made of copper, stainless steel, aluminum, nickel, titanium, combusted carbon, copper, or stainless steel or aluminum-cadmium alloys treated with carbon, nickel, titanium, silver, or the like. Furthermore, the negative electrode current collector typically has a thickness of 3 μm to 500 μm, and similar to the positive electrode current collector, tiny irregularities can be formed on its surface to improve the adhesion of the negative electrode active material. For example, negative electrode current collectors of various shapes can be used, such as films, sheets, foils, meshes, porous bodies, foams, nonwovens, and similar shapes.

[0268] The solvent can be any solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and any one of them or a mixture of two or more of them may be used. The amount of solvent used can be sufficient and is not particularly limited, provided that the coating thickness, manufacturing yield, and processability of the negative electrode material mixture are taken into account.

[0269] (3) partition

[0270] The lithium secondary battery according to the present invention includes a separator between the positive electrode and the negative electrode.

[0271] The separator isolates the positive and negative electrodes and provides a path for the movement of lithium ions. Any separator can be used without particular limitation, as long as it is generally used as a separator in a lithium secondary battery. In particular, separators with high moisture retention capacity for electrolyte solutions and low resistance to electrolyte ion transport can be used.

[0272] In particular, porous polymer membranes, such as those prepared from polyolefin-based polymers like ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or laminated structures having two or more of the aforementioned porous polymer membranes, can be used. Additionally, typical porous nonwovens, such as nonwovens formed from high-melting-point glass fibers or polyethylene terephthalate fibers, can be used. Furthermore, separators coated with ceramic components or polymer materials can be used to ensure heat resistance or mechanical strength, and separators with single-layer or multi-layer structures can optionally be used.

[0273] The lithium secondary batteries described above according to the present invention can be suitably used in portable devices (such as mobile phones, laptops and digital cameras) and electric vehicles (such as hybrid electric vehicles (HEVs)).

[0274] Therefore, according to another embodiment of the present invention, a battery module including a lithium secondary battery as a unit battery and a battery pack including the battery module are provided.

[0275] Battery modules or battery packs can be used as a power source for at least one of the following medium and large-sized devices: power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or energy storage systems.

[0276] The shape of the lithium secondary battery of the present invention is not particularly limited, but cylindrical, prismatic, pouch or coin-shaped lithium secondary batteries using cans can be used.

[0277] The lithium secondary battery according to the present invention can be used not only in battery cells used as power sources for small devices, but also as unit batteries in medium and large battery modules comprising multiple battery cells.

[0278] The present invention will now be described in detail with reference to specific embodiments. However, the following embodiments are merely illustrative and the scope of the invention is not limited thereto. It will be apparent to those skilled in the art that various modifications and substitutions may be made within the scope and spirit of the invention. These modifications and substitutions fall within the scope of the claims included herein.

[0279] [Example]

[0280] Example 1.

[0281] (Preparation of precursor compositions for the preparation of polymer electrolytes)

[0282] After adding 5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 0.05 g of the compound represented by Formula 2-3, and 0.2 g of the polymerization initiator (2,2'-azobis(iso-butyronitrile), AIBN) to 94.75 g of a non-aqueous organic solvent (in which ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), and propyl propionate (PP) are mixed in a volume ratio of 20:10:20:50), LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0283] (Preparation of secondary batteries)

[0284] A positive electrode mixture slurry was prepared by adding 96 parts by weight of LiCoO2 as the positive electrode active material, 2 parts by weight of carbon black as the conductive agent, and 2 parts by weight of polyvinylidene fluoride (PVDF) as the binder to N-methyl-2-pyrrolidone (NMP) as the solvent. The positive electrode mixture slurry was then coated onto a 20 μm thick aluminum (Al) film serving as the positive electrode current collector, dried, and then rolled to prepare the positive electrode.

[0285] A negative electrode slurry was prepared by mixing graphite (as the negative electrode active material), styrene-butadiene rubber (as the binder), CMC (as the thickener), and carbon black (as the conductive agent) in a weight ratio of 96.3:1:1.5:1.2, and then adding NMP (as the solvent). The negative electrode slurry was then coated onto a 10 μm thick copper (Cu) film (as the negative electrode current collector), dried, and then rolled to prepare the negative electrode.

[0286] A battery was assembled by using a positive electrode, a negative electrode, and a separator formed by three layers of polypropylene / polyethylene / polypropylene (PP / PE / PP). After injecting 5 ml of the above-prepared precursor composition for preparing the polymer electrolyte into the assembled battery, the assembled battery was allowed to stand for 2 days and then heated at 70°C for 5 hours to prepare a lithium secondary battery including the polymer electrolyte.

[0287] Example 2.

[0288] After adding 5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 20 g of the compound of Formula 2-3, and 0.2 g of the polymerization initiator (AIBN) to 74.80 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0289] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0290] Example 3.

[0291] After adding 0.5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 0.5 g of the compound of Formula 2-3, and 0.02 g of the polymerization initiator (AIBN) to 98.98 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0292] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0293] Example 4.

[0294] After adding 30 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 0.5 g of the compound of Formula 2-4, and 2.0 g of the polymerization initiator (AIBN) to 67.50 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0295] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0296] Example 5.

[0297] After adding 5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 0.05 g of the compound of Formula 2-7, and 0.2 g of the polymerization initiator (AIBN) to 94.75 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0298] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0299] Example 6.

[0300] After adding 40 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 0.5 g of the compound of Formula 2-7, and 2.5 g of the polymerization initiator (AIBN) to 57 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0301] Then, an attempt was made to prepare a lithium secondary battery in the same manner as in Example 1, except that the precursor composition for preparing the polymer electrolyte prepared above was used. However, the battery could not be operated because it was difficult to prepare a uniform polymer electrolyte and the considerable amount of oligomers contained therein dissolved unevenly in the non-aqueous organic solvent.

[0302] Comparative Example 1.

[0303] LiPF6 was dissolved in 100g of a non-aqueous organic solvent (a mixture of ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), and propyl propionate (PP) in a volume ratio of 20:10:20:50) to prepare a 1M concentration of LiPF6, thereby preparing a non-aqueous electrolyte solution. Then, a lithium secondary battery was prepared in the same manner as in Example 1, except that the above-described non-aqueous electrolyte solution was used (see Table 1 below).

[0304] Compare Example 2.

[0305] After adding 5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol) and 0.2 g of the polymerization initiator (AIBN) to 94.80 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0306] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0307] Comparative Example 3.

[0308] After adding 24 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol) and 1.5 g of the polymerization initiator (AIBN) to 74.50 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0309] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0310] Comparative Example 4.

[0311] After adding 50 g of the compound of formula 2-7 to 50.0 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0312] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0313] Comparative Example 5.

[0314] After adding 5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 50 g of the compound of Formula 2-7, and 0.2 g of the polymerization initiator (AIBN) to 44.8 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of polymer electrolytes (see Table 1 below).

[0315] In addition to using the precursor composition for preparing polymer electrolytes prepared above, lithium secondary batteries were prepared in the same manner as in Example 1.

[0316] Comparative Example 6.

[0317] The lithium secondary battery was prepared in the same manner as in Example 1, except that an acrylate phosphate compound of Formula 3 was used instead of the oligomer of Formula 1 to prepare the precursor composition for the preparation of the polymer electrolyte.

[0318] [Formula 3]

[0319]

[0320] Compare Example 7.

[0321] Except that, after dissolving LiPF6 in 94.775 g of a non-aqueous organic solvent to achieve a LiPF6 concentration of 1 M, a precursor composition for preparing a polymer electrolyte was prepared by adding 5.0 g of an oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 0.025 g of a compound of Formula 2-3, and 0.2 g of a polymerization initiator (AIBN), the lithium secondary battery was prepared in the same manner as in Example 1.

[0322] Compare Example 8.

[0323] Except that, after adding 0.5 g of the oligomer represented by Formula 1A-2 (n2 and m2 are 10, k2 is 2, and the weight-average molecular weight (Mw) is 3,000 g / mol), 2.5 g of the compound of Formula 2-3, and 0.02 g of the polymerization initiator (AIBN) to 96.88 g of a non-aqueous organic solvent, LiPF6 was dissolved to a concentration of 1 M to prepare a precursor composition for the preparation of a polymer electrolyte, the lithium secondary battery was prepared in the same manner as in Example 1.

[0324] [Table 1]

[0325]

[0326]

[0327] [Experimental Example]

[0328] Experimental Example 1. Viscosity Assessment

[0329] The viscosity of the precursor compositions for preparing polymer electrolytes prepared in Examples 1 to 3 and 5, and the precursor compositions for preparing polymer electrolytes prepared in Comparative Examples 1 to 3, 6 and 7, was measured using a Brookfield Rheometer DV-III. The measurement results are shown in Table 2 below.

[0330] [Table 2]

[0331] Viscosity (25℃ / cPs) Example 1 4.8 Example 2 3.8 Example 3 3.5 Example 5 4.6 Comparative Example 1 3.5 Comparative Example 2 5.2 Comparative Example 3 10< Comparative Example 6 5.1 Comparative Example 7 5.0

[0332] Referring to Table 2, regarding the viscosity of the precursor compositions for preparing polymer electrolytes in Examples 1 to 3 and 5 of the present invention, it can be seen that the viscosity is lower than that of the precursor compositions for preparing polymer electrolytes in Comparative Examples 2 and 3 that only include oligomers of Formula 1, the precursor composition for preparing polymer electrolytes in Comparative Example 6 that includes oligomers of Formula 3, or the precursor composition for preparing polymer electrolytes in Comparative Example 7 that includes a slightly smaller amount of oligomers of Formula 2.

[0333] As can be seen, the viscosity of the precursor composition for preparing polymer electrolytes of Example 2, which has a higher amount of the compound of Formula 2, and the precursor composition for preparing polymer electrolytes of Example 3, which has a lower amount of the oligomer of Formula 1, is similar to the viscosity of the non-aqueous electrolyte solution in the liquid electrolyte solution state of Comparative Example 1.

[0334] Experimental Example 2. Stability Assessment

[0335] The secondary batteries prepared in Examples 1 to 5 and the secondary batteries prepared in Comparative Examples 1 to 8 were fully charged to 100% state of charge (SOC) at 4.45V. These batteries were then stored in a chamber at 85°C (heating rate: 5°C / 1 minute) for 8 hours to examine the increase in thickness (%) after high-temperature storage. The results are shown in Table 3 below.

[0336] [Table 3]

[0337] Thickness increase rate (%) after high-temperature (85℃) storage Example 1 3.0 Example 2 4.2 Example 3 4.5 Example 4 5.0 Example 5 3.2 Comparative Example 1 7.8 Comparative Example 2 10.0 Comparative Example 3 15.1 Comparative Example 4 Battery operation is not feasible Comparative Example 5 Battery operation is not feasible Comparative Example 6 9.8 Comparative Example 7 6.5 Comparative Example 8 12.3

[0338] Referring to Table 3, it can be seen that the secondary batteries of Examples 1 to 5 of the present invention have a lower thickness increase rate of 5.0% or less after high-temperature storage.

[0339] In contrast, the secondary battery of Comparative Example 1, which does not contain oligomers, showed a thickness increase of 7.8% after high-temperature storage because a larger amount of gas was generated. It can be seen that the thickness increase rate after high-temperature storage is greater than that of the secondary batteries of Examples 1 to 5 of the present invention.

[0340] Furthermore, regarding the secondary batteries of Comparative Examples 2 and 3, which include only oligomers represented by Formula 1 for preparing polymer electrolytes, the secondary battery of Comparative Example 6, which includes a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of an ... a secondary battery of an secondary battery of an secondary battery of an secondary battery of a secondary battery of an secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of an secondary battery of a secondary battery of a secondary battery of an secondary battery of a secondary battery of a secondary battery of an secondary battery of a secondary battery of a secondary battery of an secondary battery of a secondary battery of a secondary battery of a secondary battery of a secondary battery of

[0341] Regarding the secondary battery of Comparative Example 4, which uses only the compound of Formula 2 to prepare a precursor composition for polymer electrolyte, or the secondary battery of Comparative Example 5, which contains an excess of the compound of Formula 2, it can be seen that the polymer electrolyte cannot be prepared and the battery is not feasible to operate because too much electrochemical reaction of the monomer occurs.

[0342] Experimental Example 3. Discharge Capacity Assessment

[0343] Each of the secondary batteries prepared in Examples 1 to 5 and Comparative Examples 2, 3 and 6 to 8 was charged to 4.45V at 0.7C and discharged to 3V at a rate of 0.2C for initial discharge. Then, after defining the above charge and discharge as one cycle and repeating the cycle three times, the discharge efficiency of the third cycle was measured, and the results are shown in Table 4 below.

[0344] [Table 4]

[0345]

[0346]

[0347] Referring to Table 4, it can be seen that the initial discharge capacity of the secondary batteries of Examples 1 to 5 of the present invention is about 2.93 or greater, wherein the initial discharge capacity is greater than that of the secondary batteries of Comparative Examples 2, 3 and 6 to 8.

[0348] Experimental Example 4. Capacity Retention Assessment

[0349] The lithium secondary batteries prepared in Examples 1 to 5 and Comparative Examples 1 to 3 and 6 to 8 were charged / discharged at 45°C under the following conditions.

[0350] Charging conditions: 1.2C CC (constant current) / CV (constant voltage), (4.25V, 0.05C current cutoff)

[0351] Discharge conditions: 0.5C CC 3V cutoff

[0352] A cycle is defined based on one charge / discharge cycle, and after 200 cycles, the capacity retention relative to the initial state (1 cycle) is measured and listed in Table 5 below.

[0353] [Table 5]

[0354] Capacity retention rate (%) based on the 200th cycle Example 1 95 Example 2 95 Example 3 94 Example 4 96 Example 5 98 Comparative Example 1 90 Comparative Example 2 91 Comparative Example 3 >50 Comparative Example 6 88 Comparative Example 7 91 Comparative Example 8 85

[0355] Referring to Table 5, it can be seen that the capacity retention rate (%) of the secondary batteries of Examples 1 to 5 of the present invention based on the 200th cycle is about 94% or greater, wherein the capacity retention rate is greater than that of the secondary batteries of Comparative Examples 1 to 3 and 6 to 8.

Claims

1. A precursor composition for preparing a polymer electrolyte, said precursor composition comprising: Lithium salts, non-aqueous organic solvents, polymerization initiators, Oligomers represented by formula 1A, and The compound represented by formula 2, The oligomer represented by Formula 1A and the compound represented by Formula 2 comprise, in a weight ratio of 1:0.01 to 1:4: [Formula 1A] In Equation 1A, R, R1, and R2 are each independently an alkyl group having 1 to 5 carbon atoms. R' is an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted or substituted cycloalkyl group having 3 to 10 carbon atoms, an unsubstituted or substituted bicycloalkyl group having 6 to 20 carbon atoms, or an unsubstituted or substituted aryl group having 6 to 20 carbon atoms. A and A' are each independently a unit containing one or more (meth)acrylate groups, and n, m, and k are the number of repeating units. Where n is an integer from 5 to 5,000. m is an integer from 1 to 1,000, and k is an integer from 2 to 100. [Equation 2] In Equation 2, R3 is -CR5=CH2, where R5 is hydrogen or an alkyl group having 1 to 3 carbon atoms, or -R6-CF3, where R6 is an alkyl group having 1 to 20 carbon atoms and substituted with at least one fluorine atom. R4 is an alkyl or alkyl group having 1 to 20 carbon atoms and being unsubstituted or substituted with at least one fluorine atom. p is an integer of 0 or 1, and When R3 is -R6-CF3, p is 0, and R4 is an alkyl group having 1 to 20 carbon atoms that is not fluorinated.

2. The precursor composition for preparing polymer electrolytes according to claim 1, wherein, In Equation 1A, the units A and A' are each independently selected from at least one unit represented by Equations A-1 to A-6: [Formula A-1] [Formula A-2] [Formula A-3] [Formula A-4] [Formula A-5] [Formula A-6] 。 3. The precursor composition for preparing polymer electrolytes as described in claim 1, wherein R' is at least one unit selected from formulas R'-1 to R'-6: [Equation R'-1] [Equation R'-2] [Formula R'-3] [Equation R'-4] [Formula R'-5] [Formula R'-6] 。 4. The precursor composition for preparing polymeric electrolytes according to claim 1, wherein the oligomer represented by formula 1A is a compound represented by formula 1A-1: [Equation 1A-1] in, In Equation 1A-1, n1, m1, and k1 are the number of repeating units. Where n1 is an integer from 5 to 5,000. m1 is an integer from 1 to 1,000, and k1 is an integer from 1 to 100. a and a' are each an independent integer of 1 or 2, and b and b' are each an independent integer from 1 to 3.

5. The precursor composition for preparing a polymeric electrolyte as claimed in claim 1, wherein the oligomer represented by formula 1A is included in an amount from 0.1% to 30% by weight, based on the total weight of the precursor composition for preparing the polymeric electrolyte.

6. The precursor composition for preparing polymer electrolytes as described in claim 1, wherein, In Formula 2, R3 is -CR5=CH2, where R5 is hydrogen or an alkyl group having 1 to 3 carbon atoms, or -R6-CF3, where R6 is an alkyl group having 1 to 10 carbon atoms and substituted with at least one fluorine, R4 is an alkyl or alkyl group having 1 to 10 carbon atoms and not substituted with or substituted with at least one fluorine, p is an integer of 0 or 1, and when R3 is -R6-CF3, p is 0, and R4 is an alkyl group having 1 to 10 carbon atoms and not substituted with fluorine.

7. The precursor composition for preparing polymer electrolytes according to claim 1, wherein the compound represented by formula 2 is at least one compound selected from the group consisting of compounds represented by formulas 2-1 to 2-8: [Equation 2-1] [Equation 2-2] [Equation 2-3] [Equation 2-4] [Equation 2-5] [Equation 2-6] [Equation 2-7] [Equation 2-8] 。 8. The precursor composition for preparing a polymer electrolyte as claimed in claim 1, wherein, based on the total weight of the precursor composition for preparing a polymer electrolyte, it comprises from 0.01% by weight to 45% by weight of the compound represented by Formula 2.

9. A polymer electrolyte prepared by using the precursor composition for preparing a polymer electrolyte as described in claim 1.

10. A lithium secondary battery, comprising: Positive electrode; negative electrode; a partition disposed between the positive electrode and the negative electrode; And the polymer electrolyte according to claim 9.

Citation Information

Patent Citations

  • Gel polymer electrolyte composition, and gel polymer electrolyte and lithium secondary battery which comprise same

    CN111033860A

  • Block copolymers for lithium polymer batteries, electrolytes containing the same and lithium polymer batteries

    KR1020140074540A

  • KR20190062310A