A preparation method of magnesium alloy etching plate and magnesium alloy etching solution

The magnesium alloy etching plate pattern is formed through laser laser and ink jet, and the electrolytic etching process and simple components of etching liquid are used to solve the problem of time-consuming and labor-intensive photosensitive adhesive coating and narrow chemical etching window in the prior art, and magnesium alloy etching is realized The efficient and environmentally friendly production of the plates can obtain smooth and uniform etching plates and long-life etching liquid.

CN115874260BActive Publication Date: 2024-11-01BAOSTEEL METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111143299.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-28
Publication Date
2024-11-01
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

In the existing magnesium alloy etching plate production process, photosensitive adhesive coating is time-consuming and labor-intensive, raw materials are wasted, and volatile gases will be generated during the coating process, causing harm to operators and the environment. The window of the chemical etching process is narrow and difficult to control. .

Method used

Using laser laser technology to surface treatment and ink jet patterning, combined with electrolytic etching process, simple ingredient magnesium alloy etching liquid, including aliphatic carboxylic acids, aliphatic carboxylic acid esters, fatty amines and surfactants, etching liquid temperature and current Density is easy to control.

Benefits of technology

The rapid and labor-saving preparation of magnesium alloy etching plates is achieved, which reduces raw material waste and volatile gas generation, expands the process window, improves production efficiency, and the obtained etching plate surface is smooth and the slope is uniform, extending the service life of the etching liquid.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A preparation method of a magnesium alloy etching plate and a magnesium alloy etching solution, the preparation method comprising: 1) surface treatment, placing a magnesium alloy plate with a clean surface into a laser machine to radiate a desired pattern, the laser power is 10-20W, and the laser point spacing is 0.01-0.05mm; 2) preparation of a pre-coated plate, using a UV ink jet device to spray photosensitive glue on the pattern area radiated by laser to form a spray pattern, and then photocuring the spray pattern to obtain a magnesium alloy pre-coated plate; 3) electrolytic etching, using a graphite electrode as a cathode and a magnesium alloy pre-coated plate as an anode, and placing it in an electrolytic tank filled with etching solution for electrolytic etching. The preparation method has a wide etching process window, and the process parameters are easy to control. The overall process is time-saving and labor-saving, easy to operate, and can avoid harm to the operator's body and pollution to the surrounding environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnesium alloy etching, and in particular to a preparation method of a magnesium alloy etching plate and a magnesium alloy etching solution. Background Art

[0002] As a structural / functional integrated material, magnesium alloy has the characteristics of high specific strength, excellent thermal conductivity, easy solubility and good damping performance. It has broad application prospects in aerospace, rail transportation, 3C products, biomedicine and printing industries.

[0003] In the printing industry, magnesium alloy etching plates have the advantages of small specific gravity, fast heat dissipation, high surface hardness, easy demoulding, and high printing durability compared with zinc alloy etching plates and copper alloy etching plates. At the same time, magnesium alloy, as a green and environmentally friendly material, has a low degree of damage to the environment. It has gradually replaced zinc and copper plates and become the main raw material for the production of etching plates.

[0004] The traditional production process of magnesium alloy etching plate is as follows: the photosensitive adhesive is coated on the surface of the clean magnesium alloy plate by roller coating or screen printing, and the film with the pattern is laid flat on the surface of the dry photosensitive adhesive layer. After irradiation with ultraviolet light, the photosensitive adhesive under the transparent part of the film undergoes a photochemical reaction, so that the water-soluble photosensitive adhesive is converted into an acid-resistant, alkali-resistant and water-resistant organic curing layer, and the non-transparent part of the film can be washed away in a weak alkaline solution because it has not undergone a photochemical reaction. Then, the magnesium alloy plate (pre-coated plate) with the organic curing layer pattern is placed in the etching equipment. Under certain temperature and stirring speed conditions, the stirring paddle sprinkles the etching solution composed of nitric acid and additives on the surface of the magnesium alloy plate, and forms a three-dimensional pattern on the surface of the magnesium alloy plate by chemical corrosion (etching). The role of the acid is to remove the metal magnesium, and the role of the additive is to inhibit corrosion protection and reduce side corrosion.

[0005] Chinese patent CN107699895A discloses "an etching process for a magnesium alloy etching plate", which uses chemical etching to prepare a magnesium alloy etching plate, but the process window of etching speed and etching temperature is narrow.

[0006] Chinese patent CN108437647A discloses "a method for producing a magnesium alloy etching plate using a protective film instead of a back anti-corrosion paint", which uses roller coating or screen printing to apply photosensitive adhesive, and the process is complicated.

[0007] Chinese patent CN102839376A discloses "Preparation and application of magnesium or magnesium alloy etching additives", which are composed of the following chemical substances by weight percentage: carboxylic acid ester or carboxylic acid or a mixture of carboxylic acid ester and carboxylic acid is 10-60%, alkane is 5-40%, surfactant is 2-25%, defoamer is 0.01-2%, viscosity enhancer is 0.01-2%, and distilled water is the balance. However, its composition is complex, and the etching solution is only for chemical etching.

[0008] In the current production process of magnesium alloy etched plates, the coating of photosensitive adhesive is time-consuming and labor-intensive, with a large amount of raw material waste. In addition, volatile gases are generated during the coating process, causing harm to the operator's body and pollution to the surrounding environment. In addition, the existing preparation methods of magnesium alloy etched plates all use chemical etching, and the chemical etching method of stirring and splashing etching liquid has a narrow process window. Summary of the invention

[0009] The purpose of the present invention is to provide a preparation method of a magnesium alloy etching plate and a magnesium alloy etching liquid. The formation of patterns in the preparation process of the magnesium alloy etching plate is more time-saving and labor-saving, and the raw materials are fully utilized; the etching process window is wide, and the process parameters are easy to control; the overall process is time-saving and labor-saving, easy to operate, and the generation of volatile gases is avoided, the harm to the operator's body and the pollution to the surrounding environment are reduced, and the production efficiency of the magnesium alloy etching plate is improved; at the same time, an etching liquid with simple composition and long service life is proposed for the electrolytic etching of magnesium alloys, so that the frequent replacement of the etching liquid during the etching process is avoided.

[0010] To achieve the above purpose, the technical solution of the present invention is as follows:

[0011] A method for preparing a magnesium alloy etching plate comprises the following steps:

[0012] 1) Surface treatment

[0013] Put the cleaned magnesium alloy plate into the laser machine to laser out the required pattern, the laser power is 10-20W, and the laser point spacing is 0.01-0.05mm;

[0014] 2) Preparation of pre-coated panels

[0015] Using ink jetting equipment to jet UV ink on the pattern area emitted by laser to form a jet pattern, and then photocuring the jet pattern to obtain a magnesium alloy pre-coated sheet;

[0016] 3) Electrolytic etching

[0017] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode, which are placed in an electrolytic cell containing etching solution for electrolytic etching.

[0018] Preferably, the magnesium alloy sheet is magnesium alloy AZ31, magnesium alloy AZ33 or magnesium alloy AZ41.

[0019] Preferably, the resin in the UV ink is epoxy acrylate, polyester acrylate or acrylic urethane.

[0020] Preferably, in step 2), the light curing power is 2-3 kW, the temperature is 25-30° C., and the humidity is 30-40%.

[0021] Preferably, in step 3), the distance between the graphite electrode and the magnesium alloy pre-coated plate is 5 to 15 cm, the etching solution temperature is 25 to 45° C., and the current density is 1 to 5 A / dm 2 .

[0022] The present invention adopts the method of laser surface treatment + spraying UV ink to form a target pattern on the surface of the magnesium alloy plate to prepare the pre-coated plate. The target pattern is first laser-projected on the surface of the magnesium alloy plate, and then the UV ink is sprayed onto the pattern surface using ink jetting equipment. The original preparation of the pre-coated plate is to apply photosensitive adhesive by roller coating or screen printing, and then lay the film with the pattern printed on it on the surface of the dry photosensitive adhesive layer. After irradiation with ultraviolet light, the photosensitive adhesive under the light-transmitting part of the film undergoes a photochemical reaction, so that the water-soluble photosensitive adhesive is converted into an acid-resistant, alkali-resistant and water-resistant organic solidified layer. Compared with the traditional method, the method of forming a pattern on the surface of the magnesium alloy plate of the present invention saves time and effort in the preparation process, fully utilizes raw materials, and can avoid the generation of volatile gases during the coating process, reducing physical harm to operators and pollution to the surrounding environment.

[0023] The pattern formed on the surface of the magnesium alloy pre-coated plate of the present invention has strong adhesion because the target pattern is laser-projected on the surface of the magnesium alloy plate and then UV ink is sprayed. The laser changes the microscopic morphology of the magnesium alloy surface, improves the adhesion of the UV ink on the magnesium alloy surface, and can make the pattern better adhere to the magnesium alloy plate, so as to obtain a pre-coated plate with better pattern adhesion, and can avoid the UV ink falling off due to too low adhesion during the etching process, and the occurrence of side etching and other phenomena. The slope of the magnesium alloy etched plate finally obtained is smooth, the slope is uniform, and the surface has no pitting. After the traditional pre-coated plate is etched, the 0.05mm line has broken points or jagged edges, while the 0.02mm line of the pre-coated plate of the present invention is still clearly visible after etching, indicating that the pattern of the present invention has better adhesion on the magnesium alloy.

[0024] The present invention obtains a pre-coated plate with strong pattern adhesion, and then uses an electrolytic etching process to prepare a magnesium alloy etched plate. In the traditional chemical etching process for preparing magnesium alloy etched plates, the etching solution temperature and etching time need to be precisely controlled. If it is too high, the magnesium alloy etched plate will be too thin or even perforated. If it is too low, the etching depth is not enough to meet the requirements. In the electrolytic etching process of the present invention, the etching solution temperature is controlled at 25-45°C, and the current density is controlled at 1-5A / dm 2 , can obtain etched plates with smooth slope, uniform slope and no pitting on the surface. The parameter control is relatively wide, the process parameters are easy to control, and it is easier to obtain magnesium alloy etched plates with smooth slope, uniform slope and no pitting on the plate surface.

[0025] The present invention also provides a magnesium alloy etching solution used in the method for preparing the magnesium alloy etching plate. The magnesium alloy etching solution comprises, by weight percentage, 0.6-1.2% aliphatic carboxylic acid, 1-1.5% aliphatic carboxylic acid ester, 0.8-1.3% aliphatic amine, 0.5-1% surfactant, 0.5-1% organic solvent, 10-25% inorganic acid, and the rest is water.

[0026] Preferably, the aliphatic carboxylic acid is selected from one or more of n-hexanoic acid, n-octanoic acid, 2,2-dimethylhexanoic acid, 2,3-dimethylhexanoic acid, and 2-ethylhexanoic acid.

[0027] Preferably, the aliphatic carboxylic acid ester is selected from one or more of propyl dodecanoate, isopropyl dodecanoate and ethyl dodecanoate.

[0028] Preferably, the fatty amine is one or more of octylamine, undecylamine and dodecylamine.

[0029] Preferably, the surfactant is one or both of fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether.

[0030] Preferably, the organic solvent is one or more of ethyl acetate, petroleum ether and dioxane.

[0031] Preferably, the inorganic acid is nitric acid or sulfuric acid.

[0032] In the magnesium alloy etching solution composition design of the present invention:

[0033] The present invention aims at preparing a magnesium alloy etching plate by electrolytic etching, and for the first time proposes a magnesium alloy etching solution suitable for electrolytic etching, wherein when aliphatic carboxylic acids, aliphatic carboxylic acid esters and aliphatic amines contained in the magnesium alloy etching solution are electrolyzed in an acidic solution, the aliphatic carboxylic acids, aliphatic carboxylic acid esters and aliphatic amines have a corrosion inhibition function and can be uniformly adsorbed on the surface of the magnesium alloy, thereby inhibiting rapid corrosion and side corrosion of the magnesium alloy, achieving a uniform etching effect, and thus obtaining an etching plate with a uniform surface pattern slope.

[0034] Surfactants can make organic substances with corrosion inhibition function such as aliphatic carboxylic acids, aliphatic carboxylic acid esters and aliphatic amines dispersed evenly and effectively in the etching solution, and can also regulate the corrosion rate of magnesium alloys and the smoothness of the corrosion slope.

[0035] Since the magnesium alloy etching solution of the present invention contains organic substances such as aliphatic carboxylic acids, aliphatic carboxylic acid esters, fatty amines, surfactants, and inorganic acids, adding a small amount of organic solvents can make the various components in the etching solution fully and evenly dissolved together. Since the added aliphatic carboxylic acids, aliphatic carboxylic acid esters, and fatty amines are all organic substances with fewer branches, these organic substances have a smaller negative impact on the chemical activity of inorganic acids, can delay the decline in acid reaction activity, and extend the service life of the etching solution. Therefore, the same volume of etching solution can etch more magnesium alloys, and the etching solution does not need to be frequently replaced, further improving production efficiency. For example, using the process of the present invention, the activity of the etching solution decreases when the magnesium content in 60L magnesium alloy etching solution reaches more than 9kg, while in traditional chemical etching, the activity of the etching solution decreases when the magnesium content in 60L etching solution reaches 7-8kg.

[0036] Beneficial effects of the present invention:

[0037] 1. In the preparation process of the magnesium alloy etched plate of the present invention, the pattern on the magnesium alloy pre-coated plate is formed by laser surface treatment + spraying UV ink, while the pattern formation on the traditional magnesium alloy pre-coated plate needs to go through roller coating or screen printing, film pasting, light curing and alkali washing, etc. The pattern formation process on the magnesium alloy pre-coated plate of the present invention is more time-saving and labor-saving than the traditional process, and the raw materials are fully utilized, which can avoid the generation of volatile gases during the coating process, reduce the harm to the operator's body and the pollution to the surrounding environment; and the pattern formed on the surface of the magnesium alloy pre-coated plate obtained by the present invention has strong adhesion, which can avoid the UV ink from falling off during the etching process, the occurrence of side etching and the like, and finally obtain a magnesium alloy etched plate with a smooth slope, uniform slope and no pitting on the plate surface.

[0038] 2. The present invention adopts electrolytic etching to prepare magnesium alloy etched plates. Compared with the existing preparation method of magnesium alloy etched plates, the process window is wide, the process parameters are easy to control, and it is easier to obtain magnesium alloy etched plates with smooth slopes, uniform slopes, and no pitting on the plate surface.

[0039] 3. The overall magnesium alloy etching plate process of the present invention adopts laser surface treatment + spraying UV ink + electrolytic etching, which simplifies the production process flow compared with the traditional etching plate preparation process (roll coating or screen printing + film pasting + light curing + alkali washing + chemical etching, etc.), improves the production efficiency of the magnesium alloy etching plate, and the production efficiency is increased by about 20%, which has obvious social and economic benefits.

[0040] 4. The present invention is aimed at the preparation of magnesium alloy etching plates and proposes for the first time a magnesium alloy etching solution suitable for electrolytic etching of magnesium alloys, wherein aliphatic carboxylic acids, aliphatic carboxylic acid esters, and fatty amines with corrosion inhibition function are added to the magnesium alloy etching solution, and aliphatic carboxylic acids, aliphatic carboxylic acid esters, and fatty amines are all organic substances with fewer branches. These organic substances have less negative impact on the chemical activity of inorganic acids, can delay the decline in acid reaction activity, and extend the service life of the etching solution. Therefore, the same volume of etching solution can etch more magnesium alloys, and the etching solution does not need to be frequently replaced, which further improves production efficiency.

[0041] 5. The present invention is directed to the preparation of an etching solution for magnesium alloy etching plates by electrolytic etching, which has simple ingredients and readily available raw materials, whereas the existing etching solution used for magnesium alloy chemical etching contains at least a dozen ingredients and is relatively complex. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with the embodiments.

[0043] Embodiment 1 A method for preparing an AZ31 magnesium alloy etching plate comprises the following steps:

[0044] 1) Surface treatment

[0045] Place the cleaned AZ31 magnesium alloy sheet into the laser machine to laser out the required pattern. The laser power is 10W and the laser point spacing is 0.04mm.

[0046] 2) Preparation of pre-coated panels

[0047] The ink jetting device is used to jet UV ink on the pattern area emitted by the laser to form a jetting pattern, and then the jetting pattern is photocured to obtain a magnesium alloy pre-coated plate; the UV ink resin is acrylic urethane, the photocuring power is 3kW, the temperature is 25°C, and the humidity is 30%;

[0048] 3) Electrolytic etching

[0049] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode. The plates are placed in an electrolytic tank containing an etching solution for electrolytic etching. The etching solution comprises the following components by weight: 0.8% octanoic acid, 1.2% isopropyl dodecanoate, 0.8% dodecylamine, 0.7% fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, 0.8% ethyl acetate, 15.7% nitric acid, and the rest is water. The distance between the graphite electrode and the magnesium alloy pre-coated plate is 12 cm, the etching solution temperature is 35°C, and the current density is 3A / dm 2 .

[0050] The obtained magnesium alloy etching plate has a pattern slope of 100-105 degrees, a uniform slope, and no pits on the plate surface, which meets the requirements of hot stamping printing.

[0051] In the electrolytic etching process of this embodiment, when the amount of magnesium dissolved in 60L magnesium alloy etching solution reaches 9.5kg, the activity of the etching solution begins to decrease. When the magnesium alloy etching plate has uneven slope, smooth surface, side etching or pitting, it means that the activity of the etching solution begins to decrease.

[0052] Embodiment 2 The preparation method of AZ31 magnesium alloy etching plate comprises the following steps:

[0053] 1) Surface treatment

[0054] Place the cleaned AZ31 magnesium alloy sheet into a laser machine to laser out the desired pattern. The laser power is 15W and the laser point spacing is 0.03mm.

[0055] 2) Preparation of pre-coated panels

[0056] The ink jetting device is used to jet UV ink on the pattern area emitted by the laser to form a jetting pattern, and then the jetting pattern is photocured to obtain a magnesium alloy pre-coated plate; the UV ink resin is epoxy acrylate, the photocuring power is 2.5kW, the temperature is 27°C, and the humidity is 39%;

[0057] 3) Electrolytic etching

[0058] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode. The plates are placed in an electrolytic tank containing an etching solution for electrolytic etching. The etching solution comprises the following components by weight: 1% n-octanoic acid, 1.3% isopropyl dodecanoate, 1.2% undecylamine, 0.8% fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, 0.7% ethyl acetate, 17% nitric acid, and the rest is water. The distance between the graphite electrode and the magnesium alloy pre-coated plate is 8 cm, the etching solution temperature is 30°C, and the current density is 2.5 A / dm 2 .

[0059] The obtained magnesium alloy etching plate pattern has a slope of 90-105 degrees, a uniform slope, and no pits on the plate surface, which meets the requirements of hot stamping printing.

[0060] In the electrolytic etching process of this embodiment, when the amount of magnesium dissolved in 60L of magnesium alloy etching solution reaches 9.3kg, the activity of the etching solution begins to decrease.

[0061] Embodiment 3 The preparation method of AZ33 magnesium alloy etching plate comprises the following steps:

[0062] 1) Surface treatment

[0063] Place the cleaned AZ33 magnesium alloy sheet into the laser machine to laser out the required pattern. The laser power is 17W and the laser point spacing is 0.01mm.

[0064] 2) Preparation of pre-coated panels

[0065] The ink jetting device is used to jet UV ink on the pattern area emitted by the laser to form a jetting pattern, and then the jetting pattern is photocured to obtain a magnesium alloy pre-coated plate; the UV ink resin is polyester acrylate, the photocuring power is 2.8kW, the temperature is 26°C, and the humidity is 40%;

[0066] 3) Electrolytic etching

[0067] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode. The plates are placed in an electrolytic tank containing an etching solution for electrolytic etching. The etching solution components are as follows by weight: 1% 2,2-dimethylhexanoic acid, 1.2% propyl dodecanoate, 1.2% dodecylamine, 1% fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, 0.8% dioxane, 18.5% nitric acid, and the rest is water. The distance between the graphite electrode and the magnesium alloy pre-coated plate is 5 cm, the etching solution temperature is 40°C, and the current density is 1A / dm 2 .

[0068] The obtained magnesium alloy etching plate pattern has a slope of 90-110 degrees, a uniform slope, and no pits on the plate surface, which meets the requirements of hot stamping printing.

[0069] In the electrolytic etching process of this embodiment, when the amount of magnesium dissolved in 60L of magnesium alloy etching solution reaches 9.6kg, the activity of the etching solution begins to decrease.

[0070] Embodiment 4 A method for preparing an AZ33 magnesium alloy etching plate comprises the following steps:

[0071] 1) Surface treatment

[0072] Place the cleaned AZ33 magnesium alloy sheet into the laser machine to laser out the required pattern. The laser power is 20W and the laser point spacing is 0.03mm.

[0073] 2) Preparation of pre-coated panels

[0074] The ink jetting device is used to jet UV ink on the pattern area emitted by the laser to form a jetting pattern, and then the jetting pattern is photocured to obtain a magnesium alloy pre-coated plate; the UV ink resin is acrylic urethane, the photocuring power is 2kW, the temperature is 28°C, and the humidity is 36%;

[0075] 3) Electrolytic etching

[0076] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode. The plate is placed in an electrolytic cell containing an etching solution for electrolytic etching. The etching solution comprises the following components by weight: 1.1% 2,2-dimethylhexanoic acid, 1.3% ethyl dodecanoate, 1.3% octylamine, 1% fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, 0.8% dioxane, 20% nitric acid, and the rest is water. The distance between the graphite electrode and the magnesium alloy pre-coated plate is 9 cm, the etching solution temperature is 45°C, and the current density is 5A / dm 2 .

[0077] The obtained magnesium alloy etching plate pattern has a slope of 90-110 degrees, a uniform slope, and no pits on the plate surface, which meets the requirements of hot stamping printing.

[0078] In the electrolytic etching process of this embodiment, when the amount of magnesium dissolved in 60L of magnesium alloy etching solution reaches 9.1kg, the activity of the etching solution begins to decrease.

[0079] Embodiment 5 The preparation method of AZ41 magnesium alloy etching plate comprises the following steps:

[0080] 1) Surface treatment

[0081] Place the cleaned AZ41 magnesium alloy sheet into the laser machine to laser out the required pattern. The laser power is 12W and the laser point spacing is 0.02mm.

[0082] 2) Preparation of pre-coated panels

[0083] The ink jetting device is used to jet UV ink on the pattern area emitted by the laser to form a jetting pattern, and then the jetting pattern is photocured to obtain a magnesium alloy pre-coated plate; the UV ink resin is polyester acrylate, the photocuring power is 2.2kW, the temperature is 27°C, and the humidity is 32%;

[0084] 3) Electrolytic etching

[0085] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode. The plates are placed in an electrolytic tank containing an etching solution for electrolytic etching. The etching solution comprises the following components by weight: 0.6% of n-octanoic acid, 1% of isopropyl dodecanoate, 1.2% of dodecylamine, 0.9% of fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, 0.6% of ethyl acetate, 12% of nitric acid, and the rest is water. The distance between the graphite electrode and the magnesium alloy pre-coated plate is 15 cm, the temperature of the etching solution is 25°C, and the current density is 3.6 A / dm 2 .

[0086] The obtained magnesium alloy etching plate pattern has a slope of 105-115 degrees, a uniform slope, and no pits on the plate surface, which meets the requirements of hot stamping printing.

[0087] In the electrolytic etching process of this embodiment, when the amount of magnesium dissolved in 60L of magnesium alloy etching solution reaches 9.1kg, the activity of the etching solution begins to decrease.

[0088] Embodiment 6 The preparation method of AZ41 magnesium alloy etching plate comprises the following steps:

[0089] 1) Surface treatment

[0090] Place the cleaned AZ41 magnesium alloy sheet into the laser machine to laser out the required pattern. The laser power is 16W and the laser point spacing is 0.05mm.

[0091] 2) Preparation of pre-coated panels

[0092] The ink jetting device is used to jet UV ink on the pattern area emitted by the laser to form a jetting pattern, and then the jetting pattern is photocured to obtain a magnesium alloy pre-coated plate; the UV ink resin is epoxy acrylate, the photocuring power is 2.8kW, the temperature is 29°C, and the humidity is 35%;

[0093] 3) Electrolytic etching

[0094] A graphite electrode is used as a cathode and a magnesium alloy pre-coated plate is used as an anode. The plates are placed in an electrolytic tank containing an etching solution for electrolytic etching. The etching solution comprises the following components by weight: 1.2% hexanoic acid, 1% isopropyl dodecanoate, 1.3% octylamine, 0.5% fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether, 0.5% ethyl acetate, 16% nitric acid, and the rest is water. The distance between the graphite electrode and the magnesium alloy pre-coated plate is 6 cm, the etching solution temperature is 28°C, and the current density is 2.2 A / dm 2 .

[0095] The obtained magnesium alloy etching plate pattern has a slope of 90-105 degrees, a uniform slope, and no pits on the plate surface, which meets the requirements of hot stamping printing.

[0096] In the process of electrolytic etching in this embodiment, when the amount of magnesium dissolved in 60L of magnesium alloy etching solution reaches 9.7kg, the activity of the etching solution begins to decrease.

[0097] Comparative Example

[0098] The cleaned AZ31 magnesium alloy sheet substrate is laid flat on the UV ink jetting equipment, and the photosensitive adhesive is sprayed on the surface of the substrate according to the required pattern. The UV ink resin is epoxy acrylate, and then the sprayed pattern is photocured to prepare a magnesium alloy pre-coated plate. The curing power is 3kW, the temperature is 25°C, and the humidity is 30%.

[0099] 0.8% of octanoic acid, 1.2% of isopropyl dodecanoate, and 0.7% of fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether are placed in a reactor and heated to 80-100°C and kept warm for 15-30 minutes. After the solution is cooled to 40-60°C, 0.8% of ethyl acetate, 15% of nitric acid and 81.5% of water are evenly mixed together. At this point, the magnesium alloy etching solution is ready.

[0100] The above-mentioned magnesium alloy pre-coated plate (anode) and the graphite electrode (cathode) are placed in the above-mentioned magnesium alloy etching solution, the distance between the graphite electrode and the magnesium alloy pre-coated plate is 10 cm, the etching temperature is 35°C, and the current density is 3A / dm 2 , a magnesium alloy etched plate was prepared.

[0101] The slope of the etched plate pattern is less than 90°, and the slope is uneven, which does not meet the requirements for hot stamping.

[0102] Embodiments 1 to 5 of the present invention illustrate that the method and etching solution of the present invention are used to obtain a magnesium alloy etching plate with a uniform pattern slope, a smooth slope surface, and no pitting, which meets the requirements of hot stamping printing. In addition, during the electrolytic etching process, when the amount of magnesium dissolved in 60L magnesium alloy etching solution reaches more than 9kg, the activity of the etching solution decreases, indicating that the etching solution of the present invention is used in a smaller amount to obtain the same etching plate. In the comparative example, laser irradiation is not performed before UV spraying, and the etching solution composition is also different from that of the present invention. The pattern slope of the etching plate obtained is less than 90°, and the slope surface is uneven, which does not meet the requirements of hot stamping printing.

Claims

1. A method for preparing a magnesium alloy etching plate, characterized in that: The steps include: 1) Surface treatment Put the cleaned magnesium alloy plate into the laser machine to laser out the required pattern, the laser power is 10-20W, and the laser point spacing is 0.01-0.05mm; 2) Preparation of pre-coated panels Use UV ink jetting equipment to spray photosensitive glue on the laser pattern area. forming a spray pattern, and then photocuring the spray pattern to obtain a magnesium alloy pre-coated sheet; 3) Electrolytic etching Using graphite electrode as cathode and magnesium alloy pre-coated plate as anode, they are placed in an electrolytic tank filled with etching solution for electrolytic etching; The etching solution comprises, by weight percentage: aliphatic carboxylic acid: 0.6-1.2%, aliphatic carboxylic acid ester: 1-1.5%, aliphatic amine: 0.8-1.3%, surfactant: 0.5-1%, organic solvent: 0.5-1%, inorganic acid: 10-25%, and the rest is water.

2. The method for preparing a magnesium alloy etched plate according to claim 1, characterized in that: The magnesium alloy sheet is magnesium alloy AZ31, magnesium alloy AZ33 or magnesium alloy AZ41.

3. The method for preparing a magnesium alloy etched plate according to claim 1, characterized in that: The resin in the UV ink is epoxy acrylate, polyester acrylate or acrylic urethane.

4. The method for preparing a magnesium alloy etched plate according to claim 1, characterized in that: In step 2), the light curing power is 2-3 KW, the temperature is 25-30° C., and the humidity is 30-40%.

5. The method for preparing a magnesium alloy etched plate according to claim 1, characterized in that: In step 3), the distance between the graphite electrode and the magnesium alloy pre-coated plate is 5 to 15 cm, the etching solution temperature is 25 to 45°C, and the current density is 1 to 5 A / dm 2 .

6. A magnesium alloy etching solution used in the method for preparing a magnesium alloy etching plate as claimed in claim 1, characterized in that: The magnesium alloy etching solution comprises, by weight percentage, 0.6-1.2% aliphatic carboxylic acid, 1-1.5% aliphatic carboxylic acid ester, 0.8-1.3% aliphatic amine, 0.5-1% surfactant, 0.5-1% organic solvent, 10-25% inorganic acid, and the rest is water.

7. The magnesium alloy etching solution according to claim 6, characterized in that: The aliphatic carboxylic acid is selected from one or more of n-hexanoic acid, n-octanoic acid, 2,2-dimethylhexanoic acid, 2,3-dimethylhexanoic acid, and 2-ethylhexanoic acid.

8. The magnesium alloy etching solution according to claim 6, characterized in that: The aliphatic carboxylic acid ester is selected from one or more of propyl dodecanoate, isopropyl dodecanoate and ethyl dodecanoate.

9. The magnesium alloy etching solution according to claim 6, characterized in that: The fatty amine is one or more of octylamine, undecylamine and dodecylamine.

10. The magnesium alloy etching solution according to claim 6, characterized in that: The surfactant is one or both of fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether.

11. The magnesium alloy etching solution according to claim 6, characterized in that: The organic solvent is one or more of ethyl acetate, petroleum ether and dioxane.

12. The magnesium alloy etching solution according to claim 6, characterized in that: The inorganic acid is nitric acid or sulfuric acid.