A fluorination method for coal tar-based carbon material and its application in sodium ion batteries

By dispersing coal pitch and NH4PF6 in ethanol and carbonizing it at high temperature, fluorinated coal pitch-based carbon materials with low graphitization degree are prepared, which solves the problem of insufficient sodium storage capacity of sodium-ion battery negative electrode materials and achieves high capacity and good performance. Cycling performance, suitable for industrial production.

CN115893373BActive Publication Date: 2024-10-29BEIJING UNIV OF CHEM TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310024740.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-10-29
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

Existing sodium-ion batteries lack high-capacity anode materials. Commercial graphite is not suitable for sodium-ion batteries. Moreover, condensed ring aromatic hydrocarbon carbon materials have low sodium storage specific capacity after heat treatment, and there is a problem of insufficient graphitization.

Method used

Coal pitch and NH4PF6 are dispersed in ethanol, stirred at room temperature, and then carbonized at high temperature in a nitrogen atmosphere to prepare a low graphitization degree fluorinated coal pitch-based carbon material, which can be used in the negative electrode of sodium ion batteries. By regulating the surface properties of the carbon material and structure to improve sodium storage capacity.

Benefits of technology

It achieves a high sodium storage specific capacity of 450mAh g-1 as an anode material for sodium ion batteries, has both good cycle life and rate performance, reduces synthesis costs, and is suitable for industrial-scale preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115893373B_ABST
    Figure CN115893373B_ABST
Patent Text Reader

Abstract

A fluorination method for coal tar pitch-based carbon materials and its sodium ion battery application, which belongs to the field of metal ion battery negative electrode materials. Based on solid-phase heat treatment, the fluorine source and coal tar pitch are evenly mixed, and then the negative electrode carbon material is obtained by heat treatment-driven dehydrogenation and fluorination. Thanks to the structural regulation of fluorine chemistry on carbon materials, the negative electrode carbon material has a high conductivity at 0.05 A g ‑1 The ultra-high sodium storage capacity of 450 mAh g ‑1 , and has good cycle life and rate performance. The preparation method of this negative electrode material is simple, low-cost, and has excellent stability. It has the characteristics of acid-free and alkali-free treatment, laying the foundation for the large-scale preparation of sodium ion negative electrode materials, and revealing a new type of carbon material sodium storage mechanism.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of negative electrode materials for metal ion batteries, and specifically relates to a fluorination method for coal tar pitch-based carbon materials and an application thereof in sodium ion batteries. Background Art

[0002] Lithium-ion batteries are widely used in energy storage technology and power tools due to their high energy density and good cycle performance, which greatly increases the demand for lithium resources and will face the problem of lithium resource shortage in the future. Sodium-ion batteries have shown great potential in recent years due to their similar mechanism to lithium-ion batteries and abundant sodium source reserves. By learning from lithium-ion batteries, sodium-ion batteries have made rapid progress in positive electrode materials, such as polyanion compounds, layered transition metal oxides, and Prussian blue materials, while the lack of high-capacity negative electrode materials has hindered the further development of sodium-ion batteries. Commercial graphite is used as a commercial negative electrode material for lithium-ion batteries due to the lack of Na + The radius is large and it is difficult to embed into the graphite layer to form a sodium-graphite intercalation compound. Therefore, commercial graphite is not suitable for sodium-ion batteries. As an organic oligomer with a high C / H atomic ratio, polycyclic aromatic hydrocarbons are good carbon material precursors because they can generate carbon materials at a high yield under the induction of benzene rings. Converting low-cost polycyclic aromatic hydrocarbon products such as asphalt and needle coke in the coal chemical industry into high-value-added carbon negative electrode materials for sodium-ion batteries is an effective way to clean and efficiently utilize my country's coal resources. The literature (Wang et al., Chemical Engineering Journal, 2018, 342: 52–60.) records a sodium storage capacity of 272 mAh g -1 , Such asphalt and other condensed aromatic hydrocarbons are easily graphitized during heat treatment, and the prepared carbon materials exhibit a bottleneck problem of low sodium storage capacity. Summary of the invention

[0003] In order to overcome the deficiencies in the prior art, the present invention aims to provide a coal tar pitch-based sodium ion battery negative electrode carbon material with low cost, scalable preparation and low graphitization degree, as well as a preparation method and a battery. In order to achieve the above invention purpose and solve the problems in the prior art, the technical solution of the present invention is implemented as follows:

[0004] A method for preparing a fluorinated coal pitch-based carbon material for use in sodium ion batteries, the method comprising the following steps:

[0005] (1) coal tar pitch and NH4PF6 are dispersed in ethanol, stirred at room temperature and then dried to obtain solid powder A;

[0006] (2) Solid powder A is placed in a porcelain boat, placed in a tubular furnace, and nitrogen is pre-flowed to remove the air in the tube; under the protection of a nitrogen atmosphere, high-temperature carbonization is performed in a tubular furnace with a temperature holding time of 1-4 hours to prepare a fluorinated coal tar-based carbon material.

[0007] Furthermore, in step (1), the mass ratio of coal tar pitch to NH4PF6 is 1:1-1:5.

[0008] Furthermore, the carbonization temperature in step (2) is 800-1000°C; the heating rate in step (2) is 3-10°C / min. The fluorinated coal pitch-based carbon material is applied to sodium ion batteries, and the fluorinated coal pitch-based carbon material is used as a negative electrode carbon material for sodium ion batteries.

[0009] Furthermore, a method for fluorination of a coal tar pitch-based carbon material comprises the following steps:

[0010] (1) Asphalt and NH4PF6 were dispersed in 50 ml of ethanol in a certain proportion, stirred at room temperature for 3 h, and dried in an oven at 80°C for 12 h to obtain solid powder A;

[0011] (2) Solid powder A was placed in a porcelain boat, placed in a tube furnace, and nitrogen was pre-flowed for 30 min to remove the air in the tube. Under the protection of nitrogen atmosphere, high-temperature carbonization was performed in a tube furnace for 2 h to prepare F-doped carbon material.

[0012] As a preferred technical solution of the present invention, in the method for preparing the negative electrode carbon material of a sodium ion battery:

[0013] In step (1), the mass ratios of asphalt:NH4PF6 are 1:1, 1:2, 1:3, 1:4, and 1:5 respectively.

[0014] The carbonization temperature in step (2) is 800, 900, 1000°C.

[0015] The heating rates in step (2) are 3, 5, 8, and 10°C / min.

[0016] The present invention also provides a half-cell prepared by using the above-mentioned carbon material, which comprises the following steps:

[0017] Negative electrode preparation: 40 mg of negative electrode carbon material, 5 mg of carbon black, and 5 mg of sodium carboxymethyl cellulose were ground in a mortar for 20 min, 200 μL of water was added, and the mixture was ground for another 10 min to obtain a slurry. The slurry was evenly coated on the surface of copper foil with a scraper and vacuum dried at 120 ° C for 12 h to obtain a loading of 1-2 mg / cm 2 The negative electrode.

[0018] Assembly: In a glove box filled with argon, the positive electrode shell, positive electrode sheet (sodium sheet), glass fiber diaphragm, electrolyte, negative electrode sheet, and negative electrode shell were stacked in order and sealed with a sealing machine. The electrolyte used sodium perchlorate NaClO4 as the solute and ethylene carbonate EC and dimethyl carbonate DMC with a volume ratio of 1:1 as the solvent, with a concentration of 1 mol L -1 The solution was prepared by adding 5 wt% of fluoroethylene carbonate FEC as the electrolyte to complete the battery assembly.

[0019] Test: The battery test system is a blue-electric test system, and the test voltage window is 0.01-3V.

[0020] The beneficial effects of the present invention are:

[0021] (1) Fluorine chemistry was introduced into carbon materials using NH4PF6 as a fluorine source to regulate the surface properties of asphalt-derived carbon and improve the sodium storage capacity of carbon materials.

[0022] (2) During the high-temperature sintering process, NH4PF6 can attack the excess hydrogen in the asphalt to condense into carbon, greatly reducing the degree of freedom of the system. After sintering, the degree of graphitization is low, and the lower degree of graphitization is conducive to the embedding of sodium ions.

[0023] (3) Compared with other processes, this process uses low-temperature sintering, which greatly reduces the synthesis cost and is conducive to industrialization. The preparation method of this negative electrode material is simple, low-cost, and has excellent stability. It has the characteristics of acid-free and alkali-free treatment, laying the foundation for the large-scale preparation of sodium ion negative electrode materials, and at the same time reveals a new sodium storage mechanism of carbon materials.

[0024] (4) Thanks to the structural regulation of carbon materials by fluorine chemistry, the negative electrode carbon material has a high -1 The current density shows an ultra-high sodium storage capacity of 450 mAh g -1 , while also having good cycle life and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The sodium ion carbon negative electrode material prepared in Example 1-5 is 50mA·g -1 The charge and discharge curve under current density shows the optimal mass ratio of NH4PF6 to asphalt. 1, 2, 3, 4, and 5 in the figure represent the mass ratio of NH4PF6 to asphalt.

[0026] Figure 2 The sodium ion carbon negative electrode material prepared in Examples 3, 6-7 is 50 mA·g -1 The charge and discharge curves under current density show the optimal carbonization temperature.

[0027] Figure 3The sodium ion carbon negative electrode material prepared in Examples 3, 8-9 is 50mA·g -1 The charge and discharge curves under current density illustrate the optimal heating rate.

[0028] Figure 4 This is a SEM image of the sodium ion carbon negative electrode material prepared in Example 10.

[0029] Figure 5 The assembled half-cell of the sodium ion carbon negative electrode material prepared in Example 10 is at 50 mA·

[0030] g -1 Charge and discharge curves under current density.

[0031] Figure 6 The assembled half-cell of the sodium ion carbon negative electrode material prepared in Example 10 is at 2A·

[0032] g -1 Cyclic performance test results under current density.

[0033] Figure 7 The assembled half-cell of the sodium ion carbon negative electrode material prepared in Comparative Example 1 was subjected to 50 mA·

[0034] g -1 Charge and discharge curves under current density.

[0035] Figure 8 The assembled half-cell of the sodium ion carbon negative electrode material prepared in Comparative Example 2 was subjected to 50 mA·

[0036] g -1 Charge and discharge curves under current density. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with the embodiments.

[0038] Example 1

[0039] (1) 100 mg of asphalt and 100 mg of NH4PF6 were dispersed in 50 ml of ethanol, stirred at room temperature for 3 h, and dried in an oven at 80 °C for 12 h to obtain solid powder A;

[0040] (2) Solid powder A was placed in a porcelain boat, placed in a tubular furnace, and nitrogen was pre-flowed for 30 minutes to remove the air in the tube. Under the protection of nitrogen atmosphere, high-temperature carbonization was carried out in a tubular furnace at a carbonization temperature of 900°C, a holding time of 2 hours, and a heating rate of 5°C / min to prepare fluorine-doped carbon materials.

[0041] Example 2

[0042] (1) 100 mg of asphalt and 200 mg of NH4PF6 were dispersed in 50 ml of ethanol, stirred at room temperature for 3 h, and dried in an oven at 80 °C for 12 h to obtain solid powder A;

[0043] (2) Solid powder A was placed in a porcelain boat, placed in a tubular furnace, and nitrogen was pre-flowed for 30 minutes to remove the air in the tube. Under the protection of nitrogen atmosphere, high-temperature carbonization was carried out in a tubular furnace at a carbonization temperature of 900°C, a holding time of 2 hours, and a heating rate of 5°C / min to prepare fluorine-doped carbon materials.

[0044] Example 3

[0045] (1) 100 mg of asphalt and 300 mg of NH4PF6 were dispersed in 50 ml of ethanol, stirred at room temperature for 3 h, and dried in an oven at 80 °C for 12 h to obtain solid powder A;

[0046] (2) Solid powder A was placed in a porcelain boat, placed in a tubular furnace, and nitrogen was pre-flowed for 30 minutes to remove the air in the tube. Under the protection of nitrogen atmosphere, high-temperature carbonization was carried out in a tubular furnace at a carbonization temperature of 900°C, a holding time of 2 hours, and a heating rate of 5°C / min to prepare fluorine-doped carbon materials.

[0047] Example 4

[0048] (1) 100 mg of asphalt and 400 mg of NH4PF6 were dispersed in 50 ml of ethanol, stirred at room temperature for 3 h, and dried in an oven at 80 °C for 12 h to obtain solid powder A;

[0049] (2) Solid powder A was placed in a porcelain boat, placed in a tubular furnace, and nitrogen was pre-flowed for 30 minutes to remove the air in the tube. Under the protection of nitrogen atmosphere, high-temperature carbonization was carried out in a tubular furnace at a carbonization temperature of 900°C, a holding time of 2 hours, and a heating rate of 5°C / min to prepare fluorine-doped carbon materials.

[0050] Example 5

[0051] (1) 100 mg of asphalt and 500 mg of NH4PF6 were dispersed in 50 ml of ethanol, stirred at room temperature for 3 h, and dried in an oven at 80 °C for 12 h to obtain solid powder A;

[0052] (2) Solid powder A was placed in a porcelain boat, placed in a tubular furnace, and nitrogen was pre-flowed for 30 minutes to remove the air in the tube. Under the protection of nitrogen atmosphere, high-temperature carbonization was carried out in a tubular furnace at a carbonization temperature of 900°C, a holding time of 2 hours, and a heating rate of 5°C / min to prepare fluorine-doped carbon materials.

[0053] See also Figure 1, which is a charge-discharge curve of the sodium ion carbon negative electrode material prepared in Examples 1-5. By comparing the electrochemical performance of the sodium ion carbon negative electrode materials prepared in Examples 1-5, the electrochemical performance of Example 3 is the highest, at 50 mAhg -1 At a current density of 1.5 %, its specific capacity can reach 320 mAh g -1 .

[0054] Example 6

[0055] On the basis of Example 3, keeping other conditions unchanged, the carbonization temperature in step (2) of Example 3 was changed to 800° C. to prepare a sodium ion negative electrode carbon material.

[0056] Example 7

[0057] On the basis of Example 3, keeping other conditions unchanged, the carbonization temperature in step (2) in Example 3 was changed to 800° C. to prepare a negative electrode carbon material for a sodium ion battery.

[0058] See also Figure 2 , which is a charge-discharge curve of the sodium ion carbon negative electrode material prepared in Examples 3, 6-7. By comparing the sodium ion battery negative electrode carbon materials prepared in Examples 3, 6, and 7, it can be seen that the sodium ion battery negative electrode carbon material prepared under the conditions of Example 3 has the best electrochemical performance, at 50 mAh g -1 At a current density of 1.5 %, its specific capacity can reach 320 mAh g -1 .

[0059] Example 8

[0060] On the basis of Example 3, keeping other conditions unchanged, the heating rate in step (2) in Example 3 was changed to 3°C / min to prepare a sodium ion negative electrode carbon material.

[0061] Example 9

[0062] On the basis of Example 3, keeping other conditions unchanged, the heating rate in step (2) in Example 3 was changed to 8°C / min to prepare a sodium ion negative electrode carbon material.

[0063] Example 10

[0064] On the basis of Example 3, keeping other conditions unchanged, the heating rate in step (2) in Example 3 was changed to 10° C. / min to prepare a sodium ion negative electrode carbon material.

[0065] See also Figure 3, which is a charge and discharge curve diagram of the sodium ion carbon negative electrode material prepared in Examples 3, 8-10. By comparing the sodium ion battery negative electrode carbon materials prepared in Examples 3, 8, 9, and 10, it can be seen that the electrochemical performance of the sodium ion battery negative electrode carbon material prepared under the conditions of Example 10 is the best. Please refer to Figure 4 , which is the SEM morphology of the sodium ion negative electrode carbon material prepared in this embodiment. It can be seen from the figure that after high-temperature carbonization and F doping, the surface of the sodium ion negative electrode carbon material presents a porous structure.

[0066] See also Figure 5 This figure shows the half-cell assembled based on the negative electrode carbon material of the sodium ion battery in this embodiment at 50mA g -1 The charge and discharge results under current density. As shown in the figure, the current density is 50mA g -1 When the charge-discharge capacity of the electrode is 450 mAh g -1 .

[0067] See also Figure 6 , which shows the half-cell assembled based on the negative electrode carbon material of the sodium ion battery in this embodiment at 2A·g -1 Cyclic performance test results under current density. As shown in the figure, at 2A g -1 At the current density, after 1000 cycles, the capacity still remains at 300mAh g-1, the coulombic efficiency is close to 100%, and the decay rate per cycle is 0.7%.

[0068] Comparative Example 1

[0069] On the basis of Example 3, other conditions remain unchanged and the fluorine source NH4PH6 is replaced by KPF6.

[0070] Comparative Example 2

[0071] On the basis of Example 3, other conditions were kept unchanged and no F source was added.

[0072] The battery performance test results show that the sodium ion battery negative electrode carbon material provided by the present invention has excellent electrochemical properties, wherein the F element regulates the surface of the carbon material. The reason why the negative electrode carbon material of the sodium ion battery prepared with NH4PF6 as a fluorine source has better performance than KPF6 is that as the temperature rises, NH4PF6 decomposes PF6 and reacts with asphalt molecules to prepare F-doped carbon material. However, KPF6 vaporizes as the temperature rises and cannot decompose to produce PF6 molecules. Because of the presence of the F element, one site of the carbon material can store multiple sodium ions instead of the traditional single sodium ion. Based on this feature, the negative electrode carbon material of the sodium ion battery has the advantages of high specific capacity, long cycle life, and good rate performance.

Claims

1. A method for preparing a fluorinated coal pitch-based carbon material for sodium ion batteries, characterized in that: The method comprises the following steps: (1) Dispersing coal tar and NH4PF6 in ethanol, stirring at room temperature and then drying to obtain solid powder A; (2) placing solid powder A in a porcelain boat, placing it in a tubular furnace, and pre-passing nitrogen to remove the air in the tube; under the protection of nitrogen atmosphere, using the tubular furnace for high-temperature carbonization, the temperature is maintained for 1-4 hours to prepare fluorinated coal pitch-based carbon materials; In the step (1), the mass ratio of coal tar pitch to NH4PF6 is 1:1-1:

5.

2. The method for preparing a fluorinated coal pitch-based carbon material for sodium ion batteries according to claim 1, characterized in that: The carbonization temperature in step (2) is 800-1000°C.

3. The method for preparing a fluorinated coal pitch-based carbon material for sodium ion batteries according to claim 1, characterized in that: The heating rate in step (3) is 3-10°C / min.

4. The use of the fluorinated coal pitch-based carbon material prepared by the method according to claim 1, characterized in that: The fluorinated coal pitch-based carbon material is applied to sodium ion batteries, and the fluorinated coal pitch-based carbon material is used as a negative electrode carbon material for sodium ion batteries.

5. The use of the fluorinated coal pitch-based carbon material according to claim 4, characterized in that: The method for preparing the negative electrode using fluorinated coal pitch-based carbon material is as follows: Fluorinated coal pitch-based carbon material: carbon black: sodium carboxymethyl cellulose were added into a mortar at a mass ratio of 8:1:1, and water was added after grinding. The slurry was further ground to obtain a slurry. The slurry was evenly coated on the surface of the copper foil and vacuum dried to obtain a loading of 1-2 mg / cm 2 The negative electrode.

6. The use of the fluorinated coal pitch-based carbon material according to claim 5, characterized in that: The negative electrode sheet is used in the steps of assembling a battery: In a glove box filled with argon, the positive electrode shell, sodium sheet positive electrode plate, glass fiber diaphragm, electrolyte, negative electrode plate, and negative electrode shell were stacked and sealed in the order of sodium perchlorate NaClO4 as the solute and ethylene carbonate EC and dimethyl carbonate DMC with a volume ratio of 1:1 as the solvent. The concentration was 1 mol L -1 The solution was prepared by adding 5 wt % of fluoroethylene carbonate FEC as an electrolyte to complete the battery assembly.

Citation Information

Patent Citations

  • Negative active material, lithium secondary battery comprising the negative active material and manufacturing method thereof

    KR1020150103841A