Catalyst suitable for preparing primary amine compounds, catalyst preparation and catalytic method
By directly hydrothermal synthesis of Pd-Ni bimetallic nanocluster catalysts in S-1 zeolite, the problem of selectivity and low efficiency of hydrogenation reaction of nitrile compounds is solved, and high selectivity and low cost preparation of primary amines is achieved. Avoid equipment corrosion and by-product formation.
Patent Information
- Application Number
- CN202211279482.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-10-19
AI Technical Summary
The hydrogenation reaction of existing nitrile compounds has selectivity problems under mild conditions, resulting in by-products and low efficiency, and often requires additives to lead to equipment corrosion and high costs.
Direct hydrothermal synthesis method is used to prepare Pd-Ni bimetallic nanocluster catalyst PdxNi@S-1 inlaid in S-1 zeolite. Through the synergistic effect of Pd-Ni bimetallic and the zeolite constraint effect, the external amine source additive is achieved. Prepare primary amines by high selective hydrogenation.
Under mild conditions, the conversion rate of benitrile >99% and the primary amine selectivity of 92% were achieved, which reduced by-products and environmental pollution, reduced production costs, and improved the recycling of catalysts.
Smart Images

Figure CN115894142B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparing primary amine compounds by reducing nitrile compounds, and particularly relates to a method for preparing primary amine compounds by selectively hydrogenating nitrile compounds under mild conditions. Background Art
[0002] Primary amines are valuable raw materials and precursors in the production of pigments, agrochemicals, polymers, dyes, and pharmaceuticals. Several synthetic methods for primary amines have been developed over the past decades, such as reductive amination of carbonyl compounds, amination of alcohols, hydroamination of alkynes and alkenes, and hydrogenation of nitriles. Among these methods, hydrogenation of nitriles is the most economical and promising method for producing primary amines. However, due to the high reactivity of the primary aldimine intermediate, this reaction usually faces critical selectivity issues and leads to the formation of a mixture of hydrogenolysis byproducts, imines, and secondary / tertiary amine products.
[0003] Using traditional additives (such as ammonia, KHMDS, acetic acid, etc.) or using CO 2 The multiphase medium is beneficial to improve the selectivity of primary amines. However, this method will lead to equipment corrosion problems, harsh operating pressure and high cost.
[0004] Therefore, there is still an urgent need to explore efficient and stable catalysts for converting nitriles to primary amines under mild reaction conditions without any additives.
[0005] Therefore, rationally designing multi-component catalyst systems and significantly improving catalytic selectivity / activity by utilizing the synergistic effect of active metal sites of multi-metal components and optimizing the electronic state have attracted the attention of more and more researchers. Summary of the invention
[0006] Technical problem solved by the invention: The purpose of the invention is to address the problems in the above-mentioned background technology and to propose a catalytic method suitable for preparing primary amine compounds with high efficiency, stability, no corrosion to equipment, mild reaction conditions, as well as a catalyst suitable for preparing primary amine compounds and a catalyst preparation method.
[0007] Technical solution: The present invention discloses a method for preparing a catalyst suitable for preparing primary amine compounds, comprising the following steps:
[0008] Step 1: dissolving a certain amount of metal Pd salt and a certain amount of ethylenediamine in an aqueous solution, and obtaining a clear solution after ultrasonic treatment;
[0009] Step 2: dissolving a certain amount of metal Ni salt and a certain amount of ethylenediamine in an aqueous solution, and obtaining a clear solution after ultrasonic treatment;
[0010] Step 3: dissolving a certain amount of tetrapropylammonium hydroxide in a certain amount of deionized water, stirring evenly at room temperature, then adding a certain amount of tetraethyl orthosilicate to the mixed solution, and continuing to stir to obtain a mixed solution;
[0011] Step 4: Add the clarified solution obtained in step 1 and the clarified solution obtained in step 2 to the mixed solution in step 3 respectively, and stir evenly to obtain a zeolite precursor gel; transfer the zeolite precursor gel to a stainless steel autoclave and dry it to obtain a solid sample, and the solid sample is centrifuged, separated, washed, and calcined to obtain the first catalyst PdxNi@S-1, wherein x=0.1 or 0.3 or 0.6, and x represents the metal loading determined by ICP-OES.
[0012] Furthermore, the clarified solution obtained in step one is added to the mixed solution in step three and stirred evenly to obtain a zeolite precursor gel; the zeolite precursor gel is transferred to a stainless steel autoclave and dried to obtain a solid sample, and the solid sample is centrifuged, separated, washed, and calcined to obtain a second catalyst Pdy@S-1, wherein y=0.1 or 0.3 or 0.6, and y represents the metal loading determined by ICP-OES.
[0013] Further, the clarified solution obtained in step 2 is added to the mixed solution in step 3, and stirred evenly to obtain a zeolite precursor gel; the zeolite precursor gel is transferred to a stainless steel autoclave and dried to obtain a solid sample, and the solid sample is centrifuged, separated, washed, and calcined to obtain a third catalyst Ni@S-1;
[0014] Furthermore, in the step 1, the anion of the metal Pd salt is any one of a nitrate ion, a chloride ion, and a sulfate ion;
[0015] In the step 2, the anion of the metal Ni salt is any one of a nitrate ion, a chloride ion, and a sulfate ion.
[0016] Furthermore, in step 1 and step 2, the volume ratio of ethylenediamine to water is 6:1.
[0017] Furthermore, in step three, the molar ratio of tetrapropylammonium hydroxide, deionized water and tetraethyl orthosilicate is 2:35:1.
[0018] Furthermore, the calcination temperature is raised to 400-800°C at a rate of 1-5°C / min at room temperature, and the highest temperature is maintained for 1-6 hours. 2 Cool naturally to room temperature in air flow.
[0019] The invention also discloses a catalyst suitable for preparing primary amine compounds, which is prepared by the catalyst preparation method.
[0020] The present invention also discloses a catalytic method suitable for preparing primary amine compounds, comprising the above-mentioned catalyst suitable for preparing primary amine compounds; the catalyst, reaction raw materials and solvent are placed in a fixed bed reactor and sealed, the reaction temperature is set to 40-120°C, the hydrogen reaction pressure is 1-15 bar, the reaction is carried out for 0.5-3h, and after the reaction is completed and cooled to room temperature, the reaction solution is collected and filtered, and the product is identified by GC and GC-MS to determine the corresponding conversion rate and product selectivity.
[0021] Further, the reaction raw material is any one of benzonitrile, p-methylbenzonitrile, p-methoxybenzonitrile, p-fluorobenzonitrile, p-trifluorobenzonitrile, and p-chlorobenzonitrile;
[0022] The solvent is any one of methanol, ammonia methanol, ethanol, dioxane, cyclohexane and acetonitrile.
[0023] Compared with the prior art, the present invention adopts the above technical solution and has the following technical effects:
[0024] Compared with the prior art, the advantages of the present invention are: the Pd-Ni-bimetallic nanocluster catalyst PdxNi@S-1 embedded in the S-1 zeolite prepared by direct hydrothermal synthesis, the synergistic effect of the Pd-Ni bimetallic and the zeolite constraint effect significantly improve the catalyst's reaction activity for selective hydrogenation of nitrile to prepare primary amines, and under mild reaction conditions without external amine source additives, a conversion rate of benzonitrile >99% and a primary amine selectivity of 92% are achieved. The goal of highly selective hydrogenation of nitrile compounds to prepare primary amines under mild, additive-free conditions is achieved, and the problems of low efficiency of the nitrile hydrogenation process, poor product selectivity, and the need for external amine source additives are solved.
[0025] Compared with the prior art, the present method has high reaction conversion rate, high product selectivity, no amine source additives, mild conditions, and few by-products. It solves the problems of equipment corrosion and high cost in the prior art and achieves the goals of reducing environmental pollution, reducing production costs, and improving catalyst recycling. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the XRD diagram of the catalyst in the present invention. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific embodiments, which should not be construed as limiting the technical solution. Any modifications and / or changes made to the present invention will fall within the protection scope of the present invention.
[0028] Example 1
[0029] In order to further refine the preparation method of the Pd-Ni-bimetallic nanocluster catalyst, Example 1 is listed for detailed description.
[0030] The Pd-Ni-bimetallic nanocluster catalyst PdxNi@S-1 comprises the following steps:
[0031] S1. 9 mg of PdCl 2 Dissolved in 1.2 ml of aqueous solution containing 0.2 ml of ethylenediamine and then sonicated for 30 min to obtain a clear solution [Pd(NH 2 CH 2 CH 2 NH 2 ) 2 ]Cl 2 .
[0032] S2. 15 mg Ni(NO 3 ) 2 6H 2 O was dissolved in 1.2 ml of aqueous solution containing 0.2 ml of ethylenediamine and then sonicated for 30 min to obtain a clear solution [Ni(NH 2 CH 2 CH 2 NH 2 ) 3 ](NO 3 ) 2 .
[0033] S3. 16.25 g of tetrapropylammonium hydroxide (TPAOH) and 25 g of deionized water were mixed under stirring at room temperature for 10 min, and then 8.32 g of tetraethyl orthosilicate was added. After continuous stirring for 6 h to completely hydrolyze tetraethyl orthosilicate, [Pd(NH 2 CH 2 CH 2 NH 2 ) 2 ]Cl 2 solution and step (2) [Ni(NH 2 CH 2 CH 2 NH 2 ) 3 ](NO 3 ) 2 The solution was added to the mixture and stirred for 30 min. The molar composition of the resulting zeolite precursor gel was SiO 2 :TPAOH:y[Pd(NH 2 CH 2 CH 2 NH 2 ) 2 ]Cl 2 :
[0034] [Ni(NH 2 CH 2 CH 2 NH 2 ) 3 ](NO 3 ) 2 :H 2 O=1:0.4:0.00075:0.0003:35.
[0035] S4. The zeolite precursor gel in step S3 was then transferred to a 100 ml stainless steel autoclave with a Teflon liner and heated to 170 °C in a conventional oven for 72 h. The synthesized solid sample was separated by centrifugation at 9 000 rpm for 4 min, washed with deionized water, and then calcined in air at 550 °C for 6 h. The catalyst PdxNi@S-1 was obtained.
[0036] like Figure 1 As shown, it can be seen that the prepared catalyst and support S-1 have characteristic diffraction peaks of MFI molecular sieves, and there are no detectable peaks corresponding to Pd and Ni species, indicating that there are no large metal species in the synthesized samples.
[0037] Embodiment 2-6
[0038] The Pd-Ni-bimetallic nanocluster catalyst PdxNi@S-1 prepared in Example 1 was used to catalyze the hydrogenation reduction of benzonitrile, comprising the following steps: 5 mg of PdxNi@S-1, 0.5 mmol of benzonitrile and 2 mL of solvent were placed in a sealed autoclave, and 2 bar of H 2 The temperature was raised to 80°C at room temperature and maintained at 80°C for 2 hours, with a stirring rate of 400 rpm. After the reactor was cooled naturally, the mixture of the reaction liquid and the catalyst was poured out. The catalyst in the reaction liquid was fixed by magnetic force, and the clarified reaction liquid was poured out to obtain the reacted catalyst PdxNi@S-1.
[0039] The reaction products in the reaction solution were qualitatively and quantitatively analyzed by NMR and GC-MS to obtain the conversion rate of benzonitrile and the selectivity of the product primary amine.
[0040]
[0041] The purpose of this example is to study the reaction performance of the PdxNi@S-1 catalyst for selective hydrogenation of benzonitrile in different organic solvents. Through Examples 2-6, it can be found that the PdxNi@S-1 catalyst has very different hydrogenation performances for benzonitrile in different organic solvents, and the highest conversion rate and the best primary amine selectivity are obtained in ethanol solvent.
[0042] Example 7-21
[0043] The Pd-Ni-bimetallic nanocluster catalyst PdxNi@S-1 prepared in Example 1 is used to catalyze the hydrogenation reduction of benzonitrile, comprising the following steps: 5 mg PdxNi@S-1, 0.5 mmol benzonitrile and 2 mL methanol are placed in a sealed high-pressure reactor, the reaction temperature is set to 40-120°C, the hydrogen reaction pressure is 1-10 bar, the temperature is raised to 40-100°C at room temperature and maintained at 40-100°C for 0.5-4h, the stirring rate is 400rpm, and the reaction kettle is naturally cooled and the mixture of the reaction liquid and the catalyst is poured out. The catalyst in the above reaction liquid is fixed by magnetic force, and the clarified reaction liquid is poured out to obtain the reacted catalyst PdxNi@S-1.
[0044] The reaction products in the reaction solution were qualitatively and quantitatively analyzed by NMR and GC-MS to obtain the conversion rate of benzonitrile and the selectivity of the product primary amine.
[0045] The purpose of this Example 7-21 is to explore the optimal process conditions for the selective hydrogenation of benzonitrile by PdxNi@S-1 catalyst, including reaction pressure, temperature, and reaction time. Through Examples 7-21, it can be found that the optimal process conditions for the selective hydrogenation of benzonitrile by PdxNi@S-1 catalyst are mild. Under the process conditions of 2 bar, 80°C, and 2h, the conversion rate reaches more than 99%, and the primary amine selectivity is 92%.
[0046]
[0047]
[0048] Examples 22-26
[0049] The Pd-Ni-bimetallic nanocluster catalyst PdxNi@S-1 prepared in Example 1 is used to catalyze the hydrogenation reduction of benzonitrile, comprising the following steps: 5 mg of PdxNi@S-1, 0.5 mmol of reaction raw materials and 2 mL of methanol are placed in a sealed high-pressure reactor, the reaction temperature is set to 80°C, the hydrogen reaction pressure is 2 bar, the temperature is raised to 80°C at room temperature and maintained at 80°C for 2 hours, the stirring rate is 400 rpm, and the reaction kettle is naturally cooled and the mixture of the reaction liquid and the catalyst is poured out. The catalyst in the above reaction liquid is fixed by magnetic force, and the clarified reaction liquid is poured out to obtain the reacted catalyst PdxNi@S-1.
[0050] The reaction products in the reaction solution were qualitatively and quantitatively analyzed by NMR and GC-MS to obtain the conversion rate of benzonitrile and the selectivity of the product primary amine.
[0051] The purpose of Examples 22-26 is to explore the reaction performance of PdxNi@S-1 catalyst for selective hydrogenation of different nitrile compounds. Through Examples 22-26, it can be found that different substitution groups have a great influence on the selective hydrogenation of nitrile compounds by PdxNi@S-1 catalyst. Methyl-substituted nitrile compounds have the best reaction effect on methyl benzonitrile, with a conversion rate of 82% and a corresponding primary amine selectivity of 99%.
[0052]
[0053]
[0054] The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations, and any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst suitable for preparing primary amine compounds, characterized in that: The following steps are included: Step 1: dissolving a certain amount of metal Pd salt and a certain amount of ethylenediamine in an aqueous solution, and obtaining a clear solution after ultrasonic treatment; Step 2: dissolving a certain amount of metal Ni salt and a certain amount of ethylenediamine in an aqueous solution, and obtaining a clear solution after ultrasonic treatment; Step 3: dissolving a certain amount of tetrapropylammonium hydroxide in a certain amount of deionized water, stirring evenly at room temperature, then adding a certain amount of tetraethyl orthosilicate to the mixed solution, and continuing to stir to obtain a mixed solution; Step 4: adding the clarified solution obtained in step 1 and the clarified solution obtained in step 2 to the mixed solution in step 3 respectively, and stirring evenly to obtain a zeolite precursor gel; transferring the zeolite precursor gel to a stainless steel autoclave and drying to obtain a solid sample, and subjecting the solid sample to centrifugation, separation, washing, and calcination to obtain a first catalyst PdxNi@S-1, wherein x=0.1 or 0.3 or 0.6, and x represents the metal loading determined by ICP-OES; In the step 1, the anion of the metal Pd salt is any one of a nitrate ion, a chloride ion, and a sulfate ion; In the step 2, the anion of the metal Ni salt is any one of a nitrate ion, a chloride ion, and a sulfate ion; The calcination heating method is to increase the temperature to 400-800°C at a rate of 1-5°C / min at room temperature, maintain the highest temperature for 1-6 hours, and naturally cool to room temperature in a N2 gas flow.
2. The method for preparing a catalyst suitable for preparing primary amine compounds according to claim 1, characterized in that: In the step 1 and the step 2, the volume ratio of ethylenediamine to water is 6:
1.
3. The method for preparing a catalyst suitable for preparing primary amine compounds according to claim 2, characterized in that: In the step three, the molar ratio of tetrapropylammonium hydroxide, deionized water and tetraethyl orthosilicate is 2:35:
1.
4. A catalyst suitable for preparing primary amine compounds, characterized in that: The catalyst is prepared by the catalyst preparation method described in any one of claims 1 to 3.
5. A catalytic method for preparing primary amine compounds, characterized in that: Using the catalyst according to claim 4, the catalyst, reaction raw materials, and solvent are placed in a fixed bed reactor and sealed, the reaction temperature is set to 80 ºC, the hydrogen reaction pressure is 2 bar, the reaction is carried out for 2 hours, and after the reaction is completed and cooled to room temperature, the reaction solution is collected and filtered, and the product is identified by GC and GC-MS to determine the corresponding conversion rate and product selectivity.
6. The catalytic method for preparing primary amine compounds according to claim 5, characterized in that: The reaction raw material is any one of benzonitrile, p-methylbenzonitrile, p-methoxybenzonitrile, p-fluorobenzonitrile, p-trifluorobenzonitrile and p-chlorobenzonitrile; The solvent is any one of methanol, ethanol and acetonitrile.