A high nitrogen and phosphorus core-shell flame retardant and its preparation method and application

Through the design of high-nitrogen-phosphorus core-shell flame retardants, the problems of large amounts of halogen-free flame retardants and strong hygroscopicity are solved, achieving efficient, environmentally friendly flame retardant effects and material compatibility, and reducing production costs and water absorption. Rate.

CN115895226BActive Publication Date: 2024-10-25FUZHOU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211442927.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-10-25
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

Existing halogen-free flame retardants produce less smoke and low toxicity during combustion, but large addition amounts lead to a decline in material performance. Hexachlorocyclotriphosphazene derivative flame retardants are highly hygroscopic, require harsh storage conditions, and are difficult to prepare during the preparation process. Excessive use of solvents results in wasted time and cost.

Method used

High nitrogen and phosphorus core-shell flame retardants are used. The core material is a polyphosphazene derivative derived from the reaction of urea and hexachlorocyclotriphosphazene. The shell material is polyurethane. By optimizing the reaction process and structural design, a core-shell structure is formed to improve the phase. Capacitive and flame retardant efficiency, reducing the amount of addition and production costs.

Benefits of technology

It achieves high flame retardant efficiency of flame retardants with high nitrogen and phosphorus content, good compatibility, reduced addition amount, cost saving, and reduced water absorption. It is suitable for even dispersion in the polymer matrix, and does not contain halogen elements, which is environmentally friendly and non-toxic. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115895226B_ABST
    Figure CN115895226B_ABST
Patent Text Reader

Abstract

The invention discloses a high nitrogen and phosphorus core-shell flame retardant and a preparation method and application thereof. The preparation method is: urea and hexachlorocyclotriphosphazene are dissolved in ethanol respectively, triethylamine is added to the urea solution to mix, and then the hexachlorocyclotriphosphazene solution is added to react, and the polyphosphazene flame retardant is obtained by filtering and vacuum drying, and then added to a tetrahydrofuran solution, heated to 60°C, IPDI trimer is dripped to react for 1h, and polypropylene glycol is added to continue the reaction for 2h, and then filtered and dried to obtain a high nitrogen and phosphorus core-shell flame retardant. The flame retardant is blended with PC resin, and the flame retardant effect of PC reaches UL94‑V‑0 level. The flame retardant prepared by the present invention is rich in nitrogen and phosphorus elements, has high flame retardant efficiency, and the core-shell structure isolates the flame retardant from the external environment. When the mass ratio of the core-shell material is 10:1, the water absorption rate of the flame retardant drops from 235% to 2.2%, which solves the disadvantage that the core material prepared after the reaction of urea and hexachlorocyclotriphosphazene can absorb moisture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant preparation and application, and specifically relates to a high-nitrogen-phosphorus core-shell flame retardant and a preparation method and application thereof. Background Art

[0002] Halogen-free flame retardant has attracted much attention in recent years, because halogen-containing flame retardant materials will produce a lot of smoke and toxic gases during combustion. Among halogen-free flame retardants, intumescent flame retardants (IFRs) have the advantages of less smoke and low toxicity, and are one of the most widely used halogen-free flame retardants. Most intumescent flame retardants are added in large amounts, which often causes a sharp decline in material performance. In the preparation process of hexachlorocyclotriphosphazene derivative flame retardants, the hydrochloric acid and acid binding agent generated in the reaction system will generate hydrochloride insoluble in the reaction solvent and mix with the product, so after the reaction is completed, a large amount of solvent is needed for further purification, resulting in a waste of time and cost. In addition, although the flame retardant prepared from hexachlorocyclotriphosphazene and urea has a high nitrogen and phosphorus content, due to the extremely strong hygroscopicity of urea itself, the flame retardant prepared from it has a strong hygroscopicity at room temperature, and the storage conditions are harsh, and it needs to be dried before use. Summary of the invention

[0003] The object of the present invention is to develop a kind of high nitrogen and phosphorus core-shell flame retardant without halogen elements, the flame retardant has high flame retardant efficiency and small addition amount, compared with the mainstream ammonium polyphosphate intumescent flame retardant on the market, the flame retardant prepared by the present invention has good compatibility with polymer, can be evenly dispersed in the polymer matrix, solves the problem of poor miscibility of APP with the matrix, and the nitrogen content in the flame retardant prepared by the present invention is up to 40wt%, and the phosphorus content is up to 30wt%. When the same flame retardant effect is achieved, the addition amount of the flame retardant of the present invention is less than half of APP. At the same time, the present invention saves time and economic cost by optimizing the manufacturing process of hexachlorocyclotriphosphazene derivative flame retardant. By making the flame retardant into a core-shell structure, the flame retardant is isolated from the external environment, and the characteristics of the strong hygroscopicity of the flame retardant prepared by the reaction of urea and hexachlorocyclotriphosphazene are overcome.

[0004] In order to achieve the above object, the present invention adopts the following technical scheme:

[0005] The structure of the high nitrogen and phosphorus core-shell flame retardant of the present invention is a core-shell type, the core material is a polyphosphazene derivative obtained by the reaction of urea and hexachlorocyclotriphosphazene, the shell material is polyurethane, the core-shell mass ratio of the flame retardant is 8-12, and the general formula of the core material structure is as follows:

[0006] ;

[0007] A method for preparing a high nitrogen and phosphorus core-shell flame retardant comprises the following steps:

[0008] (1) At room temperature, in a three-necked flask, dissolve urea in ethanol and stir to prepare a urea solution, then add a certain amount of triethylamine to the urea solution and stir evenly;

[0009] (2) Dissolve hexachlorocyclotriphosphazene in ethanol and stir to dissolve to prepare a hexachlorocyclotriphosphazene solution, then put it into a constant pressure funnel and drop it into the urea solution in the three-necked flask at a constant rate, stir and mix at 300 r / min, heat the reaction temperature to the condensation reflux temperature of the reactants, and fully react for 12 hours. After the reaction is completed, filter the reactants to remove the reaction solvent, then wash them repeatedly with ethanol three times and filter them to remove the reaction solvent and by-products, and then dry the collected precipitate in a vacuum oven for 6 hours to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content.

[0010] (3) In a three-necked flask, the polyphosphazene flame retardant powder prepared in step (2) is poured into a tetrahydrofuran solution, the rotation speed is controlled at 300-1000 r / min, the temperature is raised to 60-80° C., and then IPDI trimer is slowly added dropwise to react for 0.5-1 hour, and then polypropylene glycol is added and reacted for another 1-4 hours after the addition is complete, and then filtered, and the reactant is placed in an oven at 60° C. and dried for 6 hours to obtain a core-shell type polyphosphazene flame retardant with a high nitrogen and phosphorus content, i.e., a high nitrogen and phosphorus core-shell flame retardant.

[0011] Furthermore, the amount of triethylamine added in step (1) is 2 to 3 times the molar amount of urea. Too little triethylamine will lead to insufficient reaction between urea and hexachlorocyclotriphosphazene, resulting in a decrease in the yield of the product, while too much triethylamine will cause waste.

[0012] Furthermore, the dripping time of hexachlorocyclotriphosphazene in step (2) should be between 2 and 4 hours to prevent the dripping rate from being too fast, resulting in too fast reaction rate and resulting in the increase of the particle size of the product particles. The molar ratio of urea to hexachlorocyclotriphosphazene is 3 to 4. Too low a molar ratio will lead to incomplete substitution reaction, the prepared flame retardant will contain chlorine, and the particles of the product are prone to cross-linking, and monodisperse microspheres cannot be formed. Too high a molar ratio will lead to a decrease in the content of phosphorus in the prepared flame retardant, thereby reducing the flame retardant efficiency of the flame retardant.

[0013] Furthermore, in step (3), the mass ratio of IPDI trimer to polypropylene glycol is 0.5-2, and the core-shell mass ratio of the flame retardant is 8-12.

[0014] As the preferred technical solution:

[0015] In the above step (1), in addition to ethanol as the solvent, pyridine, dimethylene sulfone, tetrahydrofuran, N,N-dimethylformamide can also be used as the solvent, and ethanol is preferred in the present invention.

[0016] The reaction temperature in the above step (2) is between 60°C and 80°C. If the reaction temperature is too high, the particle size of the product will become larger. If the reaction temperature is too low, the reaction time will be too long, affecting the preparation efficiency.

[0017] In the above step (3), in addition to using IPDI trimer as the isocyanate source, IPDI, MDI, TDI, and HDI can also be used as isocyanates to participate in the reaction. In the present invention, IPDI trimer is preferred.

[0018] In the above step (3), in addition to using polypropylene glycol as the polyol, polycaprolactone diol, polyhexamethylene adipate diol, polycarbonate diol, and polyethylene glycol can also be used as polyols to participate in the reaction. In the present invention, polypropylene glycol is preferred.

[0019] In the above implementation steps, the concentration of the hexachlorocyclotriphosphazene solution is 35-70 g / L, and the concentration of the urea solution is 18-30 g / L.

[0020] The application of the high nitrogen and phosphorus core-shell flame retardant of the present invention in the solvent-free flame retardant polyurethane adhesive is as follows: the PC is dried in a blast drying oven at 120°C for 6 hours for use to prevent the residual moisture from causing the mechanical properties of the material to deteriorate and become brittle. The pre-dried PC and the core-shell polyphosphazene flame retardant are added to the torque rheometer according to a certain mass ratio. The processing temperature is set to 220°C, the melt blending is performed for 8 minutes, and the rotor speed is 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that is uniformly mixed by melt blending, it is placed in a corresponding mold and hot-pressed at 225°C and 20MPa in a hot press. After cooling, the required test strips are obtained.

[0021] The principle of the present invention is as follows:

[0022] The chlorine atoms in the hexachlorocyclotriphosphazene used in the present invention have strong reaction activity and are easy to undergo substitution reaction with active groups such as amino groups and phenolic hydroxyl groups. In the present invention, the chlorine atoms in the hexachlorocyclotriphosphazene undergo substitution reaction with the amino groups in urea to generate hydrochloric acid. The triethylamine added in the reaction system as an acid binding agent can absorb the hydrochloric acid generated by the reaction in time, thereby promoting the reaction. With the increase of reaction time and the increase of reaction temperature, the relative molecular mass of the reactant is continuously increased, and the particle size of the product is continuously increased. After the reaction is completed, since the triethylamine hydrochloride is dissolved in the ethanol solvent, and the product polyphosphazene flame retardant is insoluble in ethanol and exists in the reaction system in the form of a precipitate, the reaction can be immediately filtered and then repeatedly washed and filtered with ethanol for 3 times. The operation is simple, and the process of using a large amount of solvent to dissolve the triethylamine hydrochloride after the reaction of preparing the hexachlorocyclotriphosphazene derivative flame retardant is omitted, which not only improves production efficiency, but also saves the cost of using solvents. Since urea easily and spontaneously absorbs water vapor in the air at room temperature, the hexachlorocyclotriphosphazene modified by urea has the hygroscopic property of urea. By adding IPDI to the outside of the prepared flame retardant core, the isocyanate group in IPDI reacts with the amine group on the surface of the flame retardant core, replacing the amine group with the isocyanate group, and then reacting with polypropylene glycol, a layer of polyurethane film is formed on its surface to form a core-shell structure, which isolates it from the external environment and greatly reduces the water absorption rate of the flame retardant.

[0023] The significant advantages of the present invention are:

[0024] (1) The flame retardant in the present invention has a small particle size of 2 to 8 μm, does not contain halogen elements, is environmentally friendly and non-toxic, and has a phosphorus content of up to 30 wt% and a nitrogen content of up to 40 wt%. The amine functional groups remaining at the end after the reaction with urea can well change the interface state of the flame retardant, so that the flame retardant can have good compatibility with the polymer matrix and be evenly dispersed in the polymer matrix. Only 4 wt% needs to be added to make the flame retardancy of PC reach UL94 V-0 level.

[0025] (2) The solvent used in the flame retardant preparation process of the present invention is ethanol, instead of the organic solvents such as tetrahydrofuran and pyridine used in the previous preparation process of hexachlorocyclotriphosphazene derivatives. Since the triethylamine hydrochloride generated by the reaction can be dissolved in the ethanol solvent, while the resultant polyphosphazene flame retardant is insoluble in ethanol and exists in the reaction system in the form of a precipitate, the product can be immediately filtered after the reaction is completed and then repeatedly washed and filtered with ethanol for three times. The operation is simple and the process of using a large amount of solvent to dissolve the triethylamine hydrochloride after the preparation of the hexachlorocyclotriphosphazene derivative flame retardant reaction is omitted. Not only the production efficiency is improved, but also the cost of using solvents is saved. Moreover, although ethanol is an organic solvent, it is not harmful to the human body, while organic solvents such as tetrahydrofuran and pyridine are physiologically toxic to the human body.

[0026] (3) Since urea can easily spontaneously absorb water vapor in the air at room temperature, the hexachlorocyclotriphosphazene modified by urea has the hygroscopic property of urea. By making the flame retardant into a core-shell structure, a layer of polyurethane film is formed on its surface, and the shell layer and the core layer are chemically bonded, the core-shell will not separate, so that it is isolated from the external environment. The water absorption rate of the flame retardant is reduced from 235% to 2.2%. If the flame retardant contains too much water during the extrusion injection molding process mixed with PC resin, it will have a harmful effect on the plastic molding process. The water in the system will vaporize at high temperature, causing defects such as bubbles, spray marks, and surface silver wires on the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the infrared spectrum of the flame retardant in Example 1;

[0028] Figure 2 This is the infrared spectrum of the flame retardant in Comparative Example 2. DETAILED DESCRIPTION

[0029] In order to better describe the performance of the high nitrogen and phosphorus core-shell flame retardant of the present invention, some specific embodiments will be further described below. It is worth noting that the following content is only an explanation of the performance of the present invention, and any improvements and adjustments made based on the present invention should be regarded as within the scope of protection of the present invention.

[0030] Test method:

[0031] (1) Water absorption test: Place 1g of sample in a constant temperature and humidity chamber, control the temperature at 25°C and the relative humidity at 50%. After 12 hours, take out and weigh. The water absorption rate of the sample is obtained by subtracting the weight before water absorption from the weight after water absorption and dividing it by the weight before water absorption.

[0032] (2) Vertical burning test: UL94 test standard is in accordance with GB / T2408-1996;

[0033] (3) Limiting oxygen index (LOI): PC samples with flame retardant added were prepared into a size of 140 mm × 6 mm × 3 mm. The flame retardant effect in nitrogen and oxygen mixed gas was measured using an HC-2 oxygen index meter (Nanjing Jiangning Analytical Instrument Factory). The flame retardant test was performed according to ASTM D2863-2000 standard.

[0034] Example 1

[0035]

[0036] (1) At room temperature, in a three-necked flask, dissolve 18 g of urea in 500 ml of ethanol and stir to prepare a urea solution. Then, add 65 g of triethylamine to the urea solution and stir evenly.

[0037] (2) 35 g of hexachlorocyclotriphosphazene was dissolved in 500 ml of ethanol and stirred to dissolve to prepare a hexachlorocyclotriphosphazene solution, which was then loaded into a constant pressure funnel and dripped into the urea solution in a three-necked flask at a constant rate within 3 hours. The mixture was stirred at 300 r / min and the temperature was raised to 60°C for sufficient reaction for 12 hours. After the reaction was completed, the reactants were filtered to remove the reaction solvent, and then washed repeatedly with ethanol three times and filtered to remove the reaction solvent and by-products. The collected precipitate was then dried in a vacuum oven for 6 hours to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content, with a yield of 96%.

[0038] (3) In a three-necked flask, 10 g of the polyphosphazene flame retardant powder prepared in step (2) was poured into 100 ml of tetrahydrofuran solution, the rotation speed was controlled at 1000 r / min, the temperature was raised to 60° C., and then 0.5 g of IPDI trimer was slowly dropped in for 1 hour, and then 0.5 g of polypropylene glycol was added in 3 portions, each time with an interval of 15 minutes. After the addition was completed, the mixture was reacted for another 2 hours, and then filtered. The reactant was placed in an oven and dried at 60° C. for 6 hours to obtain a core-shell type polyphosphazene flame retardant with a high nitrogen and phosphorus content.

[0039] (4) Dry PC in a blast drying oven at 120°C for 6 hours to prevent residual moisture from causing the mechanical properties of the material to deteriorate and become brittle. Add the pre-dried PC and core-shell polyphosphazene flame retardant into the torque rheometer at a mass ratio of 100:4. Set the processing temperature to 220°C, melt blend for 8 minutes, and the rotor speed to 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that is uniformly mixed by melt blending, put it into the corresponding mold and hot press it at 225°C and 20MPa in a hot press. After cooling, the required test specimens are obtained.

[0040] Example 2

[0041]

[0042] (1) At room temperature, in a three-necked flask, dissolve 24 g of urea in 500 ml of ethanol and stir to prepare a urea solution. Then, add 65 g of triethylamine to the urea solution and stir evenly.

[0043] (2) 35 g of hexachlorocyclotriphosphazene was dissolved in 500 ml of ethanol and stirred to dissolve to prepare a hexachlorocyclotriphosphazene solution, which was then loaded into a constant pressure funnel and dripped into the urea solution in a three-necked flask at a constant rate within 3 hours. The mixture was stirred at 300 r / min and the temperature was raised to 60°C for sufficient reaction for 12 hours. After the reaction was completed, the reactants were filtered to remove the reaction solvent, and then washed repeatedly with ethanol three times and filtered to remove the reaction solvent and by-products. The collected precipitate was then dried in a vacuum oven for 6 hours to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content, with a yield of 95%.

[0044] (3) In a three-necked flask, 10 g of the polyphosphazene flame retardant powder prepared in step (2) was poured into 100 ml of tetrahydrofuran solution, the rotation speed was controlled at 1000 r / min, the temperature was raised to 60° C., and then 0.5 g of IPDI trimer was slowly dropped in for 1 hour, and then 0.5 g of polypropylene glycol was added in 3 portions, each time with an interval of 15 minutes. After the addition was completed, the mixture was reacted for another 2 hours, and then filtered. The reactant was placed in an oven and dried at 60° C. for 6 hours to obtain a core-shell type polyphosphazene flame retardant with a high nitrogen and phosphorus content.

[0045] (4) Dry PC in a blast drying oven at 120°C for 6 hours to prevent residual moisture from causing the mechanical properties of the material to deteriorate and become brittle. Add the pre-dried PC and core-shell polyphosphazene flame retardant into the torque rheometer at a mass ratio of 100:4. Set the processing temperature to 220°C, melt blend for 8 minutes, and the rotor speed to 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that is uniformly mixed by melt blending, put it into the corresponding mold and hot press it at 225°C and 20MPa in a hot press. After cooling, the required test specimens are obtained.

[0046] Comparative Example 1

[0047]

[0048] (1) At room temperature, in a three-necked flask, dissolve 36 g of urea in 500 ml of ethanol and stir to dissolve to prepare a urea solution. Then, add 65 g of triethylamine to the urea solution and stir evenly.

[0049] (2) 35 g of hexachlorocyclotriphosphazene was dissolved in 500 ml of ethanol and stirred to dissolve to prepare a hexachlorocyclotriphosphazene solution, which was then loaded into a constant pressure funnel and dripped into the urea solution in a three-necked flask at a constant rate within 3 hours. The mixture was stirred at 300 r / min and the temperature was raised to 60°C for sufficient reaction for 12 hours. After the reaction was completed, the reactants were filtered to remove the reaction solvent, and then washed repeatedly with ethanol three times and filtered to remove the reaction solvent and by-products. The collected precipitate was then dried in a vacuum oven for 6 hours to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content, with a yield of 95%.

[0050] (3) In a three-necked flask, 10 g of the polyphosphazene flame retardant powder prepared in step (2) was poured into 100 ml of tetrahydrofuran solution, the rotation speed was controlled at 1000 r / min, the temperature was raised to 60° C., and then 0.5 g of IPDI trimer was slowly dropped in for 1 hour, and then 0.5 g of polypropylene glycol was added in 3 portions, each time with an interval of 15 minutes. After the addition was completed, the mixture was reacted for another 2 hours, and then filtered. The reactant was placed in an oven and dried at 60° C. for 6 hours to obtain a core-shell type polyphosphazene flame retardant with a high nitrogen and phosphorus content.

[0051] (4) Dry the PC in a blast drying oven at 120°C for 6 hours to prevent residual moisture from causing the mechanical properties of the material to deteriorate and become brittle. Add the pre-dried PC and core-shell polyphosphazene flame retardant into the torque rheometer at a mass ratio of 100:4. Set the processing temperature to 220°C, melt blend for 8 minutes, and the rotor speed to 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that is uniformly mixed by melt blending, put it into the corresponding mold, and hot press it at 225°C and 20MPa in a hot press. After cooling, the test strip required for the test is obtained.

[0052] Comparative Example 2

[0053]

[0054] (1) At room temperature, in a three-necked flask, dissolve 36 g of urea in 50 ml of ethanol and stir to dissolve to prepare a urea solution. Then add 65 g of triethylamine to the urea solution and stir evenly.

[0055] (2) 35 g of hexachlorocyclotriphosphazene was dissolved in 50 ml of ethanol and stirred to dissolve to prepare a hexachlorocyclotriphosphazene solution, which was then loaded into a constant pressure funnel and dripped into the urea solution in a three-necked flask at a constant rate within 3 hours. The mixture was stirred at 300 r / min and the temperature was raised to 60°C for sufficient reaction for 12 hours. After the reaction was completed, the reactants were filtered to remove the reaction solvent, and then washed three times with ethanol and filtered to remove the reaction solvent and by-products. The collected precipitate was then dried in a vacuum oven for 6 hours to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content, with a yield of 95%.

[0056] (3) Dry the PC in a blast drying oven at 120°C for 6 hours to prevent residual moisture from causing the mechanical properties of the material to deteriorate and become brittle. Add the pre-dried PC and polyphosphazene flame retardant into the torque rheometer at a mass ratio of 100:4. Set the processing temperature to 220°C, melt blend for 8 minutes, and the rotor speed to 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that is uniformly mixed by melt blending, put it into the corresponding mold, and hot press it at 225°C and 20MPa in a hot press. After cooling, the test strip required for the test is obtained.

[0057] Comparative Example 3

[0058]

[0059] (1) At room temperature, in a three-necked flask, dissolve 36 g of urea in 500 ml of ethanol and stir to dissolve to prepare a urea solution. Then, add 65 g of triethylamine to the urea solution and stir evenly.

[0060] (2) 35 g of hexachlorocyclotriphosphazene was dissolved in 500 ml of ethanol and stirred to dissolve to prepare a hexachlorocyclotriphosphazene solution, which was then loaded into a constant pressure funnel and dripped into the urea solution in a three-necked flask at a constant rate within 3 hours. The mixture was stirred at 300 r / min and the temperature was raised to 60°C for sufficient reaction for 12 hours. After the reaction was completed, the reactants were filtered to remove the reaction solvent, and then washed repeatedly with ethanol three times and filtered to remove the reaction solvent and by-products. The collected precipitate was then dried in a vacuum oven for 6 hours to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content, with a yield of 95%.

[0061] (3) In a three-necked flask, 10 g of the polyphosphazene flame retardant powder prepared in step (2) was poured into 100 ml of tetrahydrofuran solution, the rotation speed was controlled at 1000 r / min, the temperature was raised to 60° C., and then 1.0 g of IPDI trimer was slowly dropped in for 1 hour, and then 1.0 g of polypropylene glycol was added in 3 portions, each time with an interval of 15 minutes. After the addition, the mixture was reacted for another 2 hours, and then filtered. The reactant was placed in an oven and dried at 60° C. for 6 hours to obtain a core-shell type polyphosphazene flame retardant with a high nitrogen and phosphorus content.

[0062] (4) Dry the PC in a blast drying oven at 120°C for 6 hours to prevent residual moisture from causing the mechanical properties of the material to deteriorate and become brittle. Add the pre-dried PC and core-shell polyphosphazene flame retardant into the torque rheometer at a mass ratio of 100:4. Set the processing temperature to 220°C, melt blend for 8 minutes, and the rotor speed to 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that is uniformly mixed by melt blending, put it into the corresponding mold, and hot press it at 225°C and 20MPa in a hot press. After cooling, the test strip required for the test is obtained.

[0063] Comparative Example 4

[0064] The PC was dried in a blast drying oven at 120°C for 6 hours to prevent the residual moisture from reducing the mechanical properties of the material and making it brittle. The pre-dried PC and ammonium polyphosphate flame retardant were added to the torque rheometer at a mass ratio of 100:4. The processing temperature was set to 220°C, melt blending was performed for 8 minutes, and the rotor speed was 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that was uniformly mixed by melt blending, it was placed in the corresponding mold and hot-pressed at 225°C and 20MPa in a hot press. After cooling, the required test strips were obtained.

[0065] Comparative Example 5

[0066] The PC was dried in a blast drying oven at 120°C for 6 hours to prevent residual moisture from reducing the mechanical properties of the material and making it brittle. The pre-dried PC and ammonium polyphosphate flame retardant were added to the torque rheometer at a mass ratio of 100:8. The processing temperature was set to 220°C, melt blending was performed for 8 minutes, and the rotor speed was 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that was uniformly mixed by melt blending, it was placed in the corresponding mold and hot-pressed at 225°C and 20MPa in a hot press. After cooling, the required test strips were obtained.

[0067] Comparative Example 6

[0068] The PC was dried in a blast drying oven at 120°C for 6 hours to prevent residual moisture from reducing the mechanical properties of the material and making it brittle. The pre-dried PC and ammonium polyphosphate flame retardant were added to the torque rheometer at a mass ratio of 100:12. The processing temperature was set to 220°C, melt blending was performed for 8 minutes, and the rotor speed was 60r / min. After obtaining a PC / polyphosphazene flame retardant composite material block that was uniformly mixed by melt blending, it was placed in the corresponding mold and hot-pressed at 225°C and 20MPa in a hot press. After cooling, the required test strips were obtained.

[0069] Performance Testing

[0070] 1. The flame retardants and flame retardant PC prepared in the examples and comparative examples were tested for performance, and the results are shown in Tables 1 and 2 (for example, the determination methods of the technical indicators of the present invention are all standard methods used in the art).

[0071]

[0072]

[0073] Since urea easily absorbs water vapor in the air spontaneously at room temperature, the hexachlorocyclotriphosphazene substituted by urea has the characteristic of urea hygroscopicity. It can be found from the data of Table 1 for comparison and embodiment that by adding IPDI outside the prepared flame retardant core, the isocyanate group in IPDI reacts with the amine group on the surface of the flame retardant core, and the amine group is replaced by the isocyanate group, and then reacts with polypropylene glycol to form a layer of polyurethane film on its surface, forming a core-shell structure to separate it from the external environment, so except for comparative example 2, the water absorption rate of the flame retardant is greatly reduced. And comparative example 2 is directly in contact with the external environment due to the lack of protection of the core-shell structure, and is easily absorbed when exposed to the environment, with a water absorption rate of up to 235%. At the same time, it can be seen from Example 1, Comparative Example 2, and Comparative Example 3 that the core-shell structure causes the particle size of the flame retardant to increase. When the core-shell mass ratio decreases, the particle size gradually increases due to the easy occurrence of cross-linking reaction between the particles.

[0074] From the flame retardant test of PC in Table 2, it is found that adding 4wt% of the prepared flame retardant can make the flame retardant effect of PC reach UL94 V-0, while if ammonium polyphosphate is used as the flame retardant, 12wt% is required to achieve the flame retardant effect of the flame retardant prepared in the present invention. And from the flame retardant test of PC in Example 1, Example 2, and Comparative Example 1, it can be found that during the preparation of the flame retardant, when the proportion of urea increases, the flame retardant performance of the flame retardant will decrease. This is because the urea content in the flame retardant increases, resulting in a decrease in phosphorus content, an increase in nitrogen content, and a deterioration in flame retardant performance.

[0075] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for preparing a high nitrogen and phosphorus core-shell flame retardant, characterized in that: The structure of the flame retardant is a core-shell type, the core material is a polyphosphazene derivative obtained by reacting urea and hexachlorocyclotriphosphazene, the shell material is polyurethane, and the core-shell mass ratio of the flame retardant is 8-12; the preparation thereof comprises the following steps: (1) Preparation of a polyphosphazene flame retardant with a high nitrogen and phosphorus content: at room temperature, urea is dissolved in ethanol and stirred to dissolve to prepare a urea solution, and triethylamine is added to the urea solution and stirred evenly; then a hexachlorocyclotriphosphazene solution composed of hexachlorocyclotriphosphazene and ethanol is added dropwise, and the mixture is stirred at 300 r / min, and the temperature is heated to the condensation reflux temperature of the reactants. After the reaction is completed, the reactants are filtered to remove the reaction solvent, and then repeatedly washed with ethanol three times and filtered to remove the reaction solvent and by-products, and then the collected precipitate is vacuum dried to obtain a white polyphosphazene flame retardant with a high nitrogen and phosphorus content; (2) pouring the polyphosphazene flame retardant prepared in step (1) into a tetrahydrofuran solution, controlling the rotation speed to 300-1000 r / min, raising the temperature to 60-80°C, and then slowly dripping IPDI trimer to react for 0.5-1h, then adding polypropylene glycol, and reacting for another 1-4h, filtering and drying to obtain a high nitrogen and phosphorus core-shell flame retardant; In step (1), the reaction temperature of urea and hexachlorophosphazene is 60-80°C, and the reaction time is 12-24h; The added amount of the flame retardant accounts for 4wt% to 8wt% of the mass fraction of the PC resin.

2. The method for preparing a high nitrogen and phosphorus core-shell flame retardant according to claim 1, characterized in that: In step (1), the molar ratio of urea to hexachlorocyclotriphosphazene is 3-4, and the amount of triethylamine is 2-3 times the molar amount of urea.

3. The method for preparing a high nitrogen and phosphorus core-shell flame retardant according to claim 1, characterized in that: In step (2), the mass ratio of IPDI trimer to polypropylene glycol is 0.5-2.

4. The method for preparing a high nitrogen and phosphorus core-shell flame retardant according to claim 1, characterized in that: In step (1), the concentration of the hexachlorocyclotriphosphazene solution is 35-70 g / L, and the concentration of the urea solution is 18-30 g / L.

Citation Information

Patent Citations

  • Metal-loaded environment-friendly ring-crosslinked porous polyphosphazene as well as preparation method and application thereof

    CN111171324A

  • Preparation method for improving mechanical property of polyurethane flame-retardant material

    CN111978706A

  • Tannic acid-phosphazene network functionalized hydrotalcite-based flame retardant and preparation method thereof

    CN112812372A

  • Double-layer microencapsulated red phosphorus flame retardant containing cyclodextrin as well as preparation method and application of double-layer microencapsulated red phosphorus flame retardant

    CN114196074A

  • Cyclotriphosphazene flame retardant with microcapsule core-shell structure and preparation method of cyclotriphosphazene flame retardant

    CN114773681A