Infrared blocking tape

By using modified nanotin oxide antimony, nano titanium dioxide and nano copper sulfide in buildings and automotive glass, the infrared transmission problem is solved, and efficient infrared barrier and heat insulation effect is achieved, reducing energy consumption .

CN115960544BActive Publication Date: 2024-11-12DONGGUAN XIONGLIN NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211652259.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-12
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

Existing thermal insulation materials have infrared transmission problems in buildings and automotive glass, which leads to an increase in indoor temperature and increases energy consumption. Existing solutions such as metal infrared reflective layers and multi-layer thin film structural equipment have large investments and raw material costs. High and low product yield, and the thermal insulation effect of Low-E glass has room for improvement and is not decorative.

Method used

By designing the preparation materials of the substrate layer and adhesive layer, using modified nanotin antimony oxide and nanotitanium dioxide to improve infrared reflection effect, nano copper sulfide improves infrared absorption effect, and combining EVA resin and polyurethane prepolymer and other materials, it is prepared Tape with good infrared barrier effect.

Benefits of technology

The infrared barrier rate is achieved to reach 91-98%, reducing indoor temperature increases, reducing energy consumption, and improving thermal insulation performance. It is suitable for thermal insulation applications of buildings and automotive glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004011093400000151
    Figure BDA0004011093400000151
  • Figure BDA0004011093400000161
    Figure BDA0004011093400000161
Patent Text Reader

Abstract

The present invention provides an infrared blocking tape. The infrared blocking tape comprises a substrate layer and an adhesive layer which are bonded to each other; the raw materials for preparing the substrate layer comprise the following components in parts by weight: 30 to 45 parts of EVA resin, 3 to 5 parts of modified nano antimony tin oxide and 4 to 6 parts of nano titanium dioxide; the raw materials for preparing the adhesive layer comprise the following components in parts by weight: 30 to 40 parts of polyurethane prepolymer, 5 to 10 parts of curing agent, 2 to 5 parts of nano copper sulfide and 1 to 3 parts of surfactant. The infrared blocking tape provided by the present invention has a good infrared blocking effect and is suitable for use as a heat insulation and energy-saving material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat insulation materials, and in particular relates to an infrared blocking adhesive tape. Background Art

[0002] Affected by global warming, the demand for heat insulation and energy saving is increasing. Objects exposed to direct sunlight for a long time are prone to a large temperature difference between the inside and outside, making the temperature of the outer surface of the object significantly higher than the internal temperature, forming heat transfer and causing the internal temperature to rise. In order to slow down the above phenomenon, keep the inside of the object at a relatively constant temperature, and reduce the adverse effects caused by the increase in the internal temperature of the object, thermal insulation coatings used on the outer layer of buildings came into being.

[0003] CN113861785A discloses a thermal insulation coating, a preparation method of the thermal insulation coating and a thermal insulation coating. The thermal insulation coating comprises 40-60 parts of polyurethane modified acrylic emulsion, 5-10 parts of aerogel powder and 10-20 parts of polymer microspheres; the polymer microspheres are composed of porous polystyrene microspheres with a particle size of 50-100 μm and monodisperse polystyrene microspheres with a particle size of 0.02-5 μm mixed in a weight ratio of 1:(0.1-5); the thermal insulation coating is prepared from the thermal insulation coating, and the thickness of the thermal insulation coating is 1-5 mm.

[0004] CN108976950A discloses a thermal insulation paint, a thermal insulation coating and a building material. The thermal insulation paint comprises the following raw materials by weight: 20 to 40 parts of ceramic particles, 10 to 30 parts of nano aerogels, 80 to 120 parts of binders and optional additives, wherein the ceramic particles are mainly made of foamed ceramic waste. The thermal insulation paint has good thermal insulation and mechanical properties. Since both the nano aerogels and ceramic particles have microporous structures, the thermal insulation performance of the coating can be improved. Solid particles are added to the coating, and the particles can be filled into the cavities of the surface to be coated, which can reduce the amount of coating and reduce costs. The thermal insulation coating and the building material are mainly made of the above-mentioned thermal insulation paint.

[0005] In addition to heat insulation of building exterior walls, when sunlight penetrates glass windows and enters indoors, the infrared rays in the sunlight will cause the indoor temperature to rise, so ventilation or cooling devices are needed to reduce the discomfort caused by high temperatures. According to statistical results, solar radiation entering indoors through glass windows in summer significantly increases the energy consumption of air conditioners. It can be seen that the heat insulation performance of building glass windows has a great impact on indoor temperature. Similarly, the heat insulation performance of automotive glass is also one of the main factors affecting the temperature inside the car.

[0006] At present, the common heat insulation method is nothing more than setting a metal infrared reflection layer or dyeing layer on the target object. Although the metal infrared reflection layer can reflect infrared and ultraviolet rays, the related products will produce light pollution; in addition, although the dyeing layer can absorb infrared rays, its heat insulation effect is poor and it is easy to fade. In addition, there is also a heat insulation method that uses a metal coating (such as a silver coating) and a dielectric layer to form a multilayer film structure, which can selectively allow visible light to penetrate and block infrared rays through light interference; however, this method requires large equipment investment, high raw material costs and low product yield. In addition, the heat insulation effect of the existing Low-E glass still has room for improvement and is not decorative; and the glass products themselves are fragile and cannot be reworked, which has many inconveniences in application. With the large-scale use of glass windows and glass appearances (such as glass curtains) in modern buildings, as well as the rapid growth of automobile usage, the development of new heat insulation and energy-saving materials has become a technical problem that needs to be solved urgently. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an infrared blocking adhesive tape. In the present invention, by designing the raw materials for preparing the substrate layer and the adhesive layer, and further by using modified nano antimony tin oxide and nano titanium dioxide, the substrate layer has a good infrared reflection effect, and by using nano copper sulfide, the adhesive layer has a good infrared absorption effect. By using the substrate layer and the adhesive layer in combination, the prepared adhesive tape has a good infrared blocking effect and is suitable for use as a heat insulation and energy-saving material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides an infrared ray blocking adhesive tape, which comprises a substrate layer and an adhesive layer which are bonded to each other;

[0010] The raw materials for preparing the substrate layer include the following components in parts by weight: 30-45 parts of EVA resin, 3-5 parts of modified nano antimony tin oxide and 4-6 parts of nano titanium oxide;

[0011] The raw materials for preparing the adhesive layer include the following components in parts by weight: 30-40 parts of polyurethane prepolymer, 5-10 parts of curing agent, 2-5 parts of nano tungsten oxide and 1-3 parts of surfactant.

[0012] In the present invention, by designing the raw materials for preparing the substrate layer and the adhesive layer, and further by using modified nano antimony tin oxide and nano titanium dioxide, the substrate layer has a good infrared reflection effect, and by using nano copper sulfide, the adhesive layer has a good infrared absorption effect. By using the substrate layer and the adhesive layer in combination, the prepared adhesive tape has a good infrared blocking effect.

[0013] EVA resin (ethylene vinyl acetate copolymer) has good light transmittance, heat preservation and weather resistance. In the present invention, by using EVA resin as polymer particles, and by using modified nano antimony tin oxide and nano titanium dioxide in combination, and further controlling the content of modified nano antimony tin oxide and nano titanium dioxide within a specific range, an infrared blocking tape is prepared with good infrared blocking effect and heat preservation effect.

[0014] Nano copper sulfide, as a P-type semiconductor, has a strong absorption effect on near infrared. The adhesive layer prepared by the present invention has good infrared absorption effect by using nano copper sulfide and controlling its content within a specific range. If the content of nano copper sulfide is too little, its absorption effect on infrared is poor, and the infrared blocking effect of the prepared infrared blocking tape is poor; if the content of nano copper sulfide is too much, it is easy to cause cracks in the adhesive layer, which leads to poor infrared blocking effect.

[0015] In the present invention, the infrared blocking adhesive tape prepared by combining a base layer with good infrared reflection effect and an adhesive layer with good infrared absorption effect has good infrared blocking effect and good heat preservation effect.

[0016] In the present invention, the weight proportions of the EVA resin may be 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts or 45 parts, etc.

[0017] The weight proportions of the modified nano antimony tin oxide can be 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts or 5 parts.

[0018] The weight proportions of the nano titanium dioxide can be 4 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts, 5 parts, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts or 6 parts.

[0019] The weight proportions of the polyurethane prepolymer may be 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts or 40 parts, etc.

[0020] The weight proportions of the curing agent may be 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts, etc.

[0021] The weight proportions of the nano copper sulfide can be 2 parts, 2.2 parts, 2.5 parts, 2.7 parts, 3 parts, 3.3 parts, 3.6 parts, 4 parts, 4.2 parts, 4.6 parts or 5 parts.

[0022] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0023] As a preferred technical solution of the present invention, the melt index of the EVA resin is 3 to 10 g / min, for example, it can be 3 g / min, 4 g / min, 5 g / min, 6 g / min, 7 g / min, 8 g / min, 9 g / min or 10 g / min.

[0024] Preferably, the modified nano antimony tin oxide has a D 50 The particle size is 30 to 70 nm, for example, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm or 70 nm.

[0025] Preferably, the modifier of the modified nano antimony tin oxide is a silane coupling agent.

[0026] Preferably, the silane coupling agent includes hexadecyltrimethoxysilane.

[0027] In the present invention, the compatibility of the nano antimony tin oxide in the EVA resin can be improved by using the modified nano antimony tin oxide.

[0028] In the present invention, there is no special limitation on the preparation method of modified nano antimony tin oxide, and exemplary methods include but are not limited to: after uniformly mixing nano antimony tin oxide and toluene, adding a silane coupling agent thereto for modification reaction, and after the reaction is completed, centrifuging, washing, drying and grinding to obtain the modified nano antimony tin oxide.

[0029] Preferably, the D of the nano titanium dioxide 50 The particle size is 30 to 50 nm, for example, 30 nm, 32 nm, 34 nm, 36 nm, 38 nm, 40 nm, 42 nm, 44 nm, 46 nm, 48 nm or 50 nm.

[0030] As a preferred technical solution of the present invention, the raw materials for preparing the substrate layer also include 1 to 3 parts of antioxidants, for example, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts or 3 parts.

[0031] Preferably, the antioxidant is selected from any one of 2,6-di-tert-butyl-4-methylphenol, antioxidant 1U1U, triphenyl phosphite, triisodecyl phosphite, diisodecyl phenyl phosphite or dioctyl phosphite, or a combination of at least two thereof.

[0032] As a preferred technical solution of the present invention, the D 50 The particle size is 100 to 300 nm, for example, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm or 300 nm.

[0033] Preferably, the preparation method of nano copper sulfide comprises the following steps:

[0034] (1) mixing cupric chloride dihydrate and deionized water, then adding a composite sulfur source thereto, and stirring to obtain a precursor solution;

[0035] (2) placing the precursor solution in a para-polyphenylene reaction kettle to react and obtain the nano copper sulfide.

[0036] As a preferred technical solution of the present invention, the mass ratio of cupric chloride dihydrate to deionized water is 1:(100-150), for example, it can be 1:100, 1:110, 1:120, 1:130, 1:140 or 1:150, etc.

[0037] Preferably, the composite sulfur source is a mixture comprising L-cysteine ​​and thiourea.

[0038] Preferably, the molar ratio of L-cysteine ​​to thiourea is (2-4):1, for example, 2:1, 2.5:1, 3:1, 3.5:1 or 4:1.

[0039] Preferably, the mass ratio of the cupric chloride dihydrate to the composite sulfur source is 1:(1-3), for example, it can be 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8 or 1:3, etc.

[0040] Preferably, the stirring time in step (1) is 15 to 30 min, for example, it can be 15 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min.

[0041] Preferably, the reaction temperature in step (2) is 130-150°C (for example, it can be 130°C, 132°C, 134°C, 136°C, 138°C, 140°C, 142°C, 144°C, 146°C, 148°C or 150°C, etc.), and the reaction time is 7-10h (for example, it can be 7h, 7.5h, 8h, 8.5h, 9h, 9.5h or 10h, etc.).

[0042] Preferably, step (2) further includes a post-treatment step after the reaction.

[0043] Preferably, the post-treatment method includes cooling, centrifuging, washing, drying and grinding.

[0044] In the present invention, the mixing method in step (1) is ultrasound.

[0045] In the present invention, the preparation method of the nano copper sulfide specifically comprises the following steps:

[0046] (1) copper chloride dihydrate and deionized water are ultrasonically mixed, a composite sulfur source (a mixture of L-cysteine ​​and thiourea in a molar ratio of (2-4):1) is added thereto, and stirred for 15-30 minutes to obtain a precursor solution;

[0047] Wherein, the mass ratio of the cupric chloride dihydrate to deionized water is 1:(100-150), and the mass ratio of the cupric chloride dihydrate to the composite sulfur source is 1:(1-3);

[0048] (2) placing the precursor solution in a para-polyphenylene reaction kettle, reacting at 130-150° C. for 7-10 hours, cooling to room temperature, washing with anhydrous ethanol and deionized water three times respectively, placing in a vacuum drying oven for 6 hours, and grinding to obtain the nano copper sulfide.

[0049] As a preferred technical solution of the present invention, the viscosity of the polyurethane prepolymer is 3000-6000cps, for example, it can be 3000cps, 3300cps, 3600cps, 4000cps, 4200cps, 4600cps, 5000cps, 5200cps, 5500cps, 5700cps or 6000cps.

[0050] Preferably, the weight average molecular weight of the polyurethane prepolymer is 70,000 to 100,000, for example, 70,000, 72,000, 75,000, 77,000, 80,000, 83,000, 86,000, 90,000, 92,000, 95,000 or 100,000.

[0051] Preferably, the raw materials for preparing the polyurethane prepolymer include the following components in parts by weight: 40-90 parts of polyether polyol, 1-20 parts of polyester polyol, 10-20 parts of diisocyanate and 0.1-0.3 parts of catalyst A.

[0052] In the present invention, the weight proportion of the polyether polyol is 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts or 90 parts.

[0053] The weight proportions of the polyester polyol are 1 part, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts or 20 parts, etc.

[0054] The weight proportion of the diisocyanate is 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 2 parts, etc.

[0055] The weight proportion of the catalyst is 0.1 part, 0.15 part, 0.2 part, 0.25 part or 0.3 part, etc.

[0056] Preferably, the weight average molecular weight of the polyether polyol is 400-4000, for example, 400, 500, 1000, 1500, 2000, 2500, 3000, 3500 or 4000.

[0057] Preferably, the hydroxyl value of the polyether polyol is 26-88 mg KOH / g, for example, 26 mg KOH / g, 30 mg KOH / g, 40 mg KOH / g, 50 mg KOH / g, 60 mg KOH / g, 70 mg KOH / g, 80 mg KOH / g or 88 mg KOH / g.

[0058] Preferably, the weight average molecular weight of the polyester polyol is 300-4000, for example, 300, 500, 1000, 1500, 2000, 2500, 3000, 3500 or 4000.

[0059] Preferably, the polyester polyol has a hydroxyl content of 34 to 88 mg KOH / g, for example, 34 mg KOH / g, 40 mg KOH / g, 50 mg KOH / g, 60 mg KOH / g, 70 mg KOH / g, 80 mg KOH / g or 88 mg KOH / g.

[0060] Preferably, the diisocyanate is selected from toluene diisocyanate and / or hexamethylene diisocyanate, and more preferably hexamethylene diisocyanate.

[0061] Preferably, the catalyst A is an organotin catalyst.

[0062] In the present invention, the preparation method of the polyurethane prepolymer comprises the following steps:

[0063] After mixing polyether polyol, polyester polyol, diisocyanate and catalyst, a prepolymerization reaction is carried out at 75° C. to obtain a polyurethane prepolymer.

[0064] As a preferred technical solution of the present invention, the curing agent is selected from any one of dimethylolpropionic acid, trimethylolpropane or 1,6-hexanediol, or a combination of at least two thereof.

[0065] Preferably, the surfactant is selected from one or a combination of at least two of a fluorinated acrylate copolymer, a fluorinated additive, a polyester-modified hydroxyl-functional polydimethylsiloxane or an organosilicon leveling agent.

[0066] As a preferred technical solution of the present invention, the raw materials for preparing the adhesive layer also include 1 to 3 parts of infrared absorber, for example, it can be 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts or 3 parts.

[0067] Preferably, the infrared absorber is selected from infrared absorber 761 and / or infrared absorber 997.

[0068] Nano copper sulfide, as a P-type semiconductor, has a strong absorption effect on near infrared, especially has a good absorption capacity for infrared in the 1000-1500nm band, but has a poor absorption capacity for infrared above 1500nm. In the present invention, by using nano copper sulfide and an absorbent in combination, it can also have a good absorption capacity for infrared above 1500nm, further improving the infrared blocking effect of the infrared blocking tape.

[0069] Preferably, the raw materials for preparing the adhesive layer further include 0.1 to 1 part of catalyst B, for example, 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part.

[0070] Preferably, the catalyst B is selected from one or a combination of at least two of dibutyltin dilaurate, stannous isooctanoate and triethylenediamine.

[0071] As a preferred technical solution of the present invention, the thickness of the substrate layer is 1 to 3 mm, for example, it can be 1 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm or 3 mm.

[0072] As a preferred technical solution of the present invention, the thickness of the adhesive layer is 0.5-2 mm, for example, it can be 0.5 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm or 3 mm.

[0073] In the present invention, the preparation method of the infrared blocking adhesive tape is as follows:

[0074] (1) blending the raw materials for preparing the substrate layer in an internal mixer, mixing at 140 to 160° C. for 10 to 20 minutes, and then subjecting the raw materials to a vulcanizing press at 150 to 160° C. to obtain the substrate layer;

[0075] (2) After mixing the raw materials for preparing the adhesive layer, apply it to either side of the substrate layer, dry it at 80-100° C., and then compound it with the release film, roll it up, and age it at 40-50° C. for 40-72 hours to obtain the infrared blocking tape.

[0076] Compared with the prior art, the present invention has the following beneficial effects:

[0077] In the present invention, by designing the raw materials for preparing the substrate layer and the adhesive layer, further by using modified nano antimony tin oxide and nano titanium dioxide in combination and controlling the contents of the two within a specific range, and by using nano copper sulfide and controlling the content thereof within a specific range, the prepared infrared blocking tape has a good infrared blocking effect, and its infrared light blocking rate is 91-98%. After the heat insulation performance test, the ΔT is 8.7-10.5°C. DETAILED DESCRIPTION

[0078] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0079] The sources of some components in the embodiments and comparative examples are as follows:

[0080] EVA resin: Sinopec, VA-18;

[0081] Nano antimony tin oxide: Shanghai Huzheng Nano Co., Ltd.;

[0082] Nano titanium dioxide: Wuhan Xingzhongcheng Technology Co., Ltd.;

[0083] Polyether polyol: Guodu Chemical Co., Ltd., DOW-2120P, weight average molecular weight 2000, hydroxyl value 53-58 mgKOH / g;

[0084] Polyester polyol: Daicel Chemical Industries, Ltd., PCL220AL, weight average molecular weight 2000, hydroxyl value 53-59 mg KOH / g;

[0085] Organic tin catalyst: Hangzhou Guibao Chemical Co., Ltd., HG-0111

[0086] Fluorine additives: Japan DIC Corporation, F477, F553;

[0087] Silicone leveling agent: BYK-333 from BYK Chemical Company, Germany;

[0088] The preparation method of the modified nano antimony tin oxide used in the following examples and comparative examples is as follows:

[0089] After nano antimony tin oxide (4 g) and toluene (40 g) are evenly mixed, hexadecyltrimethoxysilane (2 g) is added thereto, and a modification reaction is carried out at 45° C. for 2 h, followed by centrifugation, washing with toluene 3 times, drying at 50° C. for 12 h, and then grinding to obtain the modified nano antimony tin oxide.

[0090] Example 1

[0091] This embodiment provides an infrared ray blocking tape and a preparation method thereof, wherein the infrared ray blocking tape comprises a substrate layer and an adhesive layer bonded to each other;

[0092] The raw materials for preparing the substrate layer include the following components in parts by weight: 40 parts of EVA resin, 4 parts of modified nano antimony tin oxide, 5 parts of nano titanium dioxide and 2 parts of antioxidant 1U1U;

[0093] The raw materials for preparing the adhesive layer include the following components in parts by weight: 35 parts of polyurethane prepolymer, 7 parts of trimethylolpropane, 4 parts of nano copper sulfide, 2 parts of organic silicon leveling agent, 1 part of infrared absorber 997 and 0.2 parts of dibutyltin dilaurate.

[0094] Wherein, the preparation method of nano copper sulfide is as follows:

[0095] (1) Copper chloride dihydrate and deionized water were mixed and dissolved by ultrasonication, a composite sulfur source (a mixture of L-cysteine ​​and thiourea in a molar ratio of 3:1) was added thereto, and stirred for 20 minutes to obtain a precursor solution;

[0096] Wherein, the mass ratio of cupric chloride dihydrate to deionized water is 1:120, and the mass ratio of cupric chloride dihydrate to the composite sulfur source is 1:3;

[0097] (2) placing the precursor solution in a para-polyphenylene reaction kettle, reacting at 140° C. for 8 h, cooling to room temperature, washing with anhydrous ethanol and deionized water three times respectively, placing in a vacuum drying oven for 6 h, and grinding to obtain the nano copper sulfide.

[0098] The raw materials for preparing the polyurethane prepolymer include the following components in parts by weight: 60 parts of polyether polyol, 10 parts of polyester polyol, 12 parts of hexamethylene diisocyanate and 0.2 parts of organic tin catalyst;

[0099] The preparation method of the infrared blocking adhesive tape is as follows:

[0100] (1) The raw materials for preparing the substrate layer were blended in an internal mixer, mixed at 150° C. for 15 min, and then subjected to a flat plate vulcanizer at 150° C. to obtain a substrate layer with a thickness of 2 mm;

[0101] (2) After mixing the raw materials for preparing the adhesive layer, apply it to either side of the substrate layer, dry it at 90° C., and then compound it with the release film, roll it up, and age it at 40° C. for 72 hours to obtain the infrared blocking tape, wherein the thickness of the adhesive layer is 1 mm.

[0102] Example 2

[0103] This embodiment provides an infrared ray blocking tape and a preparation method thereof, wherein the infrared ray blocking tape comprises a substrate layer and an adhesive layer bonded to each other;

[0104] The raw materials for preparing the substrate layer include the following components in parts by weight: 45 parts of EVA resin, 5 parts of modified nano antimony tin oxide, 4 parts of nano titanium dioxide and 1 part of triphenyl phosphite;

[0105] The raw materials for preparing the adhesive layer include the following components in parts by weight: 30 parts of polyurethane prepolymer, 5 parts of 1,6-hexanediol, 5 parts of nano copper sulfide, 1 part of fluorine additive, 1 part of infrared absorber 761 and 0.1 part of stannous isooctanoate.

[0106] Wherein, the preparation method of nano copper sulfide is as follows:

[0107] (1) Copper chloride dihydrate and deionized water were mixed and dissolved by ultrasonication, a composite sulfur source (a mixture of L-cysteine ​​and thiourea in a molar ratio of 2:1) was added thereto, and stirred for 15 minutes to obtain a precursor solution;

[0108] Wherein, the mass ratio of cupric chloride dihydrate to deionized water is 1:100, and the mass ratio of cupric chloride dihydrate to the composite sulfur source is 1:3;

[0109] (2) placing the precursor solution in a para-polyphenylene reaction kettle, reacting at 150° C. for 7 hours, cooling to room temperature, washing with anhydrous ethanol and deionized water three times respectively, placing in a vacuum drying oven for 6 hours, and grinding to obtain the nano copper sulfide.

[0110] The raw materials for preparing the polyurethane prepolymer include the following components in parts by weight: 90 parts of polyether polyol, 5 parts of polyester polyol, 20 parts of toluene diisocyanate and 0.3 parts of organic tin catalyst;

[0111] The preparation method of the infrared blocking adhesive tape is as follows:

[0112] (1) The raw materials for preparing the substrate layer were blended in an internal mixer, mixed at 160° C. for 10 min, and then subjected to a flat vulcanizer at 150° C. to obtain a substrate layer with a thickness of 1 mm;

[0113] (2) After mixing the raw materials for preparing the adhesive layer, apply it to either side of the substrate layer, dry it at 80° C., and then compound it with the release film, roll it up, and age it at 45° C. for 60 hours to obtain the infrared blocking tape, wherein the thickness of the adhesive layer is 0.5 mm.

[0114] Example 3

[0115] This embodiment provides an infrared ray blocking tape and a preparation method thereof, wherein the infrared ray blocking tape comprises a substrate layer and an adhesive layer bonded to each other;

[0116] The raw materials for preparing the substrate layer include the following components in parts by weight: 30 parts of EVA resin, 3 parts of modified nano antimony tin oxide, 6 parts of nano titanium dioxide and 3 parts of 2,6-di-tert-butyl-4-methylphenol;

[0117] The raw materials for preparing the adhesive layer include the following components in parts by weight: 40 parts of polyurethane prepolymer, 10 parts of dimethylol propionic acid, 2 parts of nano copper sulfide, 3 parts of organic silicon leveling agent, 3 parts of infrared absorber 761 and 1 part of dibutyltin dilaurate.

[0118] Wherein, the preparation method of nano copper sulfide is as follows:

[0119] (1) Copper chloride dihydrate and deionized water are mixed and dissolved by ultrasonication, a composite sulfur source (a mixture of L-cysteine ​​and thiourea in a molar ratio of 4:1) is added thereto, and stirred for 15 to 30 minutes to obtain a precursor solution;

[0120] Wherein, the mass ratio of cupric chloride dihydrate to deionized water is 1:150, and the mass ratio of cupric chloride dihydrate to the composite sulfur source is 1:1;

[0121] (2) placing the precursor solution in a para-polyphenylene reaction kettle, reacting at 130° C. for 10 h, cooling to room temperature, washing with anhydrous ethanol and deionized water three times respectively, placing in a vacuum drying oven for 6 h, and grinding to obtain the nano copper sulfide.

[0122] The raw materials for preparing the polyurethane prepolymer include the following components in parts by weight: 40 parts of polyether polyol, 20 parts of polyester polyol, 10 parts of hexamethylene diisocyanate and 0.1 parts of organic tin catalyst;

[0123] The preparation method of the infrared blocking adhesive tape is as follows:

[0124] (1) The raw materials for preparing the substrate layer were blended in an internal mixer, mixed at 140° C. for 20 min, and then subjected to a flat vulcanizer at 160° C. to obtain a substrate layer with a thickness of 3 mm;

[0125] (2) After mixing the raw materials for preparing the adhesive layer, apply it to either side of the substrate layer, dry it at 100° C., and then compound it with the release film, roll it up, and age it at 50° C. for 40 hours to obtain the infrared blocking tape, wherein the thickness of the adhesive layer is 2 mm.

[0126] Example 4

[0127] This embodiment provides an infrared blocking adhesive tape and a preparation method thereof, which is different from Embodiment 1 only in that:

[0128] The raw materials for preparing the substrate layer include the following components in parts by weight: 42 parts of EVA resin, 3 parts of modified nano antimony tin oxide, 4 parts of nano titanium dioxide and 2 parts of antioxidant 1U1U;

[0129] The raw materials for preparing the adhesive layer include the following components in parts by weight: 36 parts of polyurethane prepolymer, 6 parts of trimethylolpropane, 4 parts of nano copper sulfide, 2 parts of organic silicon leveling agent and 0.2 parts of dibutyltin dilaurate.

[0130] Other conditions are the same as in Example 1.

[0131] Example 5

[0132] This embodiment provides an infrared blocking tape and a preparation method thereof, which is different from Embodiment 1 only in that the raw materials for preparing the substrate layer include 3 parts of modified nano antimony tin oxide and 6 parts of nano titanium dioxide, and other conditions are the same as those in Embodiment 1.

[0133] Example 6

[0134] This embodiment provides an infrared blocking tape and a preparation method thereof, which is different from Embodiment 1 only in that the raw materials for preparing the substrate layer include 5 parts of modified nano antimony tin oxide and 4 parts of nano titanium dioxide, and other conditions are the same as those in Embodiment 1.

[0135] Example 7

[0136] This embodiment provides an infrared blocking adhesive tape and a preparation method thereof, which is different from Embodiment 1 only in that the raw material for preparing the adhesive layer contains 2 parts of nano copper sulfide, and other conditions are the same as those in Embodiment 1.

[0137] Example 8

[0138] This embodiment provides an infrared blocking adhesive tape and a preparation method thereof. The only difference from Embodiment 1 is that the raw material for preparing the adhesive layer contains 5 parts of nano copper sulfide, and other conditions are the same as those in Embodiment 1.

[0139] Comparative Example 1

[0140] This comparative example provides an infrared blocking tape and a preparation method thereof, which is different from Example 1 only in that the raw materials for preparing the substrate layer include 1 part of modified nano antimony tin oxide and 8 parts of nano titanium dioxide, and other conditions are the same as Example 1.

[0141] Comparative Example 2

[0142] This comparative example provides an infrared blocking tape and a preparation method thereof, which is different from Example 1 only in that the raw materials for preparing the substrate layer include 7 parts of modified nano antimony tin oxide and 2 parts of nano titanium dioxide, and other conditions are the same as Example 1.

[0143] Comparative Example 3

[0144] This comparative example provides an infrared blocking tape and a preparation method thereof, which is different from Example 1 only in that the weight proportion of modified nano antimony tin oxide in the preparation raw materials of the substrate layer is 9 parts, and no nano titanium dioxide is contained, and other conditions are the same as Example 1.

[0145] Comparative Example 4

[0146] This comparative example provides an infrared blocking tape and a preparation method thereof, which is different from Example 1 only in that the weight proportion of nano titanium dioxide in the preparation raw materials of the substrate layer is 9 parts, and modified nano antimony tin oxide is not contained, and other conditions are the same as Example 1.

[0147] Comparative Example 5

[0148] This comparative example provides an infrared blocking adhesive tape and a preparation method thereof, which is different from Example 1 only in that the raw material for preparing the adhesive layer contains 1 part of nano copper sulfide, and other conditions are the same as those in Example 1.

[0149] Comparative Example 6

[0150] This comparative example provides an infrared blocking adhesive tape and a preparation method thereof, which is different from Example 1 only in that 8 parts of nano copper sulfide are used as the raw material for preparing the adhesive layer, and other conditions are the same as those in Example 1.

[0151] The performance of the infrared blocking tapes provided in the above embodiments and comparative examples was tested, and the testing method was as follows:

[0152] Infrared light blocking rate: The transmittance of the infrared blocking tapes provided in the above embodiments and comparative examples was tested using an ultraviolet-visible-near infrared spectrophotometer, and the infrared light blocking rate (R NIR ):

[0153]

[0154] Where λ is the wavelength of the incident light, in nm, T(λ) is the transmittance at wavelength λ in the transmission spectrum measured by the photometer, and i(λ) is the radiation intensity at wavelength λ in the solar radiation, in Wm -2 ·nm -1 The data source is the solar radiation data in ASTMG173.

[0155] Thermal insulation performance: Use polystyrene foam boards to glue into a 20×20×20cm cubic insulation box, cut a 10×10cm opening at the top of the box, cut the infrared blocking tape provided in the above implementation and comparative examples into 12×12cm samples, and paste the samples on transparent glass, place the transparent glass at the opening (the base material layer of the sample is away from the insulation box), and make sure that the infrared blocking tape sample completely covers the opening. Use a 100W infrared lamp as the light source, and the lower surface of the infrared lamp is 40cm away from the center of the upper surface of the insulation box. When the room temperature stabilizes at the set value, turn on the infrared lamp and start timing. After 60 minutes, test the temperature in the insulation box. The test temperature is recorded as T1 (℃);

[0156] In addition, a blank control experiment was set up. The only difference from the above test was that no infrared blocking tape was set on the side of the glass away from the incubator. The other test conditions were the same as the above test process. The timing started when the infrared lamp was turned on. After 60 minutes, the temperature in the incubator was tested. The test temperature was recorded as T2 (℃).

[0157] Thermal insulation performance (△T) = T2-T1.

[0158] The performance test results of the infrared blocking tapes provided in the above examples and comparative examples are shown in Table 1 below:

[0159] Table 1

[0160]

[0161] It can be seen from the contents of Table 1 that in the present invention, by designing the raw materials for preparing the substrate layer and the adhesive layer, further by using modified nano antimony tin oxide and nano titanium dioxide in combination and controlling the contents of the two within a specific range, and by using nano copper sulfide and controlling its content within a specific range, the infrared blocking tape prepared has a good infrared blocking effect, and its infrared light blocking rate is 91-98%. After the thermal insulation performance test, ΔT is 8.7-10.5°C.

[0162] Compared with Example 1, if the content of modified nano antimony tin oxide and nano titanium dioxide is not within the specific range (Comparative Examples 1-2) or the raw materials for preparing the substrate layer do not contain modified nano antimony tin oxide or nano titanium dioxide (Comparative Examples 3-4), the infrared blocking effect of the prepared infrared blocking tape is poor.

[0163] Compared with Example 1, if the amount of nano copper sulfide used is too small (Comparative Example 5), the infrared blocking effect of the prepared infrared blocking tape is poor; if the amount of nano copper sulfide used is too large (Comparative Example 6), the adhesive layer of the prepared infrared blocking tape is prone to cracks, resulting in poor infrared blocking effect.

[0164] In summary, in the present invention, by designing the raw materials for preparing the substrate layer and the adhesive layer, further by using modified nano antimony tin oxide and nano titanium dioxide in combination and controlling the contents of the two within a specific range, and by using nano copper sulfide and controlling its content within a specific range, the infrared blocking tape prepared has a good infrared blocking effect.

[0165] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An infrared blocking adhesive tape, characterized in that: The infrared ray blocking adhesive tape comprises a substrate layer and an adhesive layer which are bonded to each other; The raw materials for preparing the substrate layer include the following components in parts by weight: 30-45 parts of EVA resin, 3-5 parts of modified nano antimony tin oxide and 4-6 parts of nano titanium dioxide; The raw materials for preparing the adhesive layer include the following components in parts by weight: 30-40 parts of polyurethane prepolymer, 5-10 parts of curing agent, 2-5 parts of nano copper sulfide and 1-3 parts of surfactant.

2. The infrared blocking tape according to claim 1, characterized in that: The melt index of the EVA resin is 3 to 10 g / min.

3. The infrared blocking tape according to claim 1, characterized in that: The modified nano antimony tin oxide D 50 The particle size is 30~70nm.

4. The infrared blocking tape according to claim 1, characterized in that: The modifier of the modified nano antimony tin oxide is a silane coupling agent.

5. The infrared blocking tape according to claim 1, characterized in that: The D 50 The particle size is 30~50nm.

6. The infrared blocking tape according to claim 1, characterized in that: The raw materials for preparing the substrate layer also include 1 to 3 parts of antioxidant.

7. The infrared blocking tape according to claim 6, characterized in that: The antioxidant is selected from any one of 2,6-di-tert-butyl-4-methylphenol, antioxidant 1U1U, triphenyl phosphite, triisodecyl phosphite, diisodecyl phenyl phosphite or dioctyl phosphite, or a combination of at least two thereof.

8. The infrared blocking tape according to claim 1, characterized in that: The D 50 The particle size is 100~300nm.

9. The infrared blocking tape according to claim 1, characterized in that: The preparation method of the nano copper sulfide comprises the following steps: (1) mixing cupric chloride dihydrate and deionized water, then adding a composite sulfur source thereto, and stirring to obtain a precursor solution; (2) placing the precursor solution in a para-polyphenylene reaction kettle to react and obtain the nano copper sulfide.

10. The infrared blocking tape according to claim 9, characterized in that: The mass ratio of the cupric chloride dihydrate to deionized water is 1:(100-150).

11. The infrared blocking tape according to claim 9, characterized in that: The composite sulfur source is a mixture of L-cysteine ​​and thiourea.

12. The infrared blocking tape according to claim 11, characterized in that: The molar ratio of L-cysteine ​​to thiourea is (2-4):

1.

13. The infrared blocking tape according to claim 9, characterized in that: The mass ratio of the cupric chloride dihydrate to the composite sulfur source is 1:(1-3).

14. The infrared blocking tape according to claim 9, characterized in that: The stirring time in step (1) is 15 to 30 minutes.

15. The infrared blocking tape according to claim 9, characterized in that: The reaction temperature in step (2) is 130-150° C., and the reaction time is 7-10 h.

16. The infrared blocking tape according to claim 9, characterized in that: After the reaction of step (2), a post-treatment step is also included.

17. The infrared blocking tape according to claim 16, characterized in that: The post-treatment method includes cooling, centrifuging, washing, drying and grinding.

18. The infrared blocking tape according to claim 1, characterized in that: The viscosity of the polyurethane prepolymer is 3000-6000 cps.

19. The infrared blocking tape according to claim 1, characterized in that: The weight average molecular weight of the polyurethane prepolymer is 70,000 to 100,000.

20. The infrared blocking tape according to claim 1, characterized in that: The raw materials for preparing the polyurethane prepolymer include the following components in parts by weight: 40-90 parts of polyether polyol, 1-20 parts of polyester polyol, 10-20 parts of diisocyanate and 0.1-0.3 parts of catalyst A.

21. The infrared blocking tape according to claim 20, characterized in that: The weight average molecular weight of the polyether polyol is 400-4000.

22. The infrared blocking tape according to claim 20, characterized in that: The hydroxyl value of the polyether polyol is 26 to 88 mg KOH / g.

23. The infrared blocking tape according to claim 20, characterized in that: The weight average molecular weight of the polyester polyol is 300-4000.

24. The infrared blocking tape according to claim 20, characterized in that: The polyester polyol has a hydroxyl content of 34 to 88 mg KOH / g.

25. The infrared blocking tape according to claim 20, characterized in that: The diisocyanate is selected from toluene diisocyanate and / or hexamethylene diisocyanate.

26. The infrared blocking adhesive tape according to claim 25, characterized in that: The diisocyanate is hexamethylene diisocyanate.

27. The infrared blocking tape according to claim 20, characterized in that: The catalyst A is an organotin catalyst.

28. The infrared blocking tape according to claim 1, characterized in that: The curing agent is selected from any one of dimethylol propionic acid, trimethylol propane or 1,6-hexanediol or a combination of at least two thereof.

29. The infrared blocking tape according to claim 1, characterized in that: The surfactant is selected from one or a combination of at least two of a fluorine-containing acrylate copolymer, a fluorine additive, a polyester-modified polydimethylsiloxane containing a hydroxyl functional group, or an organic silicon leveling agent.

30. The infrared blocking tape according to claim 1, characterized in that: The raw materials for preparing the adhesive layer also include 1 to 3 parts of infrared absorber.

31. The infrared blocking adhesive tape according to claim 30, characterized in that: The infrared absorber is selected from infrared absorber 761 and / or infrared absorber 997.

32. The infrared blocking tape according to claim 1, characterized in that: The raw materials for preparing the adhesive layer also include 0.1 to 1 part of catalyst B.

33. The infrared blocking tape according to claim 1, characterized in that: The thickness of the substrate layer is 1 to 3 mm.

34. The infrared blocking tape according to claim 1, characterized in that: The thickness of the adhesive layer is 0.5-2 mm.