A highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill and a preparation method thereof

By optimizing the chemical composition and microstructure of Cr-Mo steel, combined with special processing, the problem of fracture of Cr-Mo steel lining plates under high-hardness abrasives and impact stress has been solved, and the wear resistance and mechanical properties have been significantly improved, making it suitable for large-scale applications. scale production.

CN115961215BActive Publication Date: 2024-10-18TONGLING YOUSE JINSHEN WEAR RESISTANT MATERIAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211586161.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-18
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Cr-Mo steel lining plates are prone to fracture under working conditions with high hardness abrasives and high impact stress, and have poor wear resistance. The preparation process is complex and difficult to control, which limits its large-scale production.

Method used

It adopts high wear-resistant Cr-Mo steel lining plate for lightweight semi-autogenous grinding machine. The chemical composition is C: 0.6-1.0%, Cr: 1.5-2.5%, Ti: 1.0-2.0%, Mo: 0.5-2.0%, V :0.2-1.0%, Nb:0.03-0.09% , Si: 1.5-2.0%, P: ≤0.003%, S: ≤0.005%, the remainder is Fe and impurities, through martensite composition and embedded wear-resistant granular carbides (TiC, Mo2C, VC) and hollow structure, Combining smelting, metamorphic treatment, pouring and heat treatment processes.

Benefits of technology

It improves the wear resistance of the liner under high impact conditions, enhances the yield strength and tensile hardness, reduces casting defects, reduces production costs, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115961215B_ABST
    Figure CN115961215B_ABST
Patent Text Reader

Abstract

The invention discloses a highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill and a preparation method, and belongs to the technical field of metal material casting. The chemical components and mass percentages of the highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill are: C: 0.6-1.0%, Cr: 1.5-2.5%, Mo: 0.5-2.0%, Ti: 1.0-2.0%, V: 0.2-1.0%, Nb: 0.03-0.09%, Si: 1.5-2.0%, P: ≤0.003%, S: ≤0.005%, and the rest are Fe and unavoidable impurities. The highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill manufactured by the present invention is significantly improved in hardness, impact toughness, impact wear and other properties, and the liner does not break or deform during use, and the manufacturing process is simple and easy to operate, and is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material casting, and in particular to a highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill and a preparation method thereof. Background Art

[0002] Cr-Mo steel liner is a high-hardness alloy steel liner with excellent wear resistance that is unmatched by other materials. However, the overall stability of Cr-Mo steel liner is not strong, and casting defects are prone to occur in the thicker part during the preparation process, which eventually leads to the liner breaking when used under high-hardness abrasives and high impact stress conditions, so its abrasive wear resistance cannot be fully utilized.

[0003] At present, the performance of traditional Cr-Mo steel can hardly meet the actual application requirements because the lining plates of large semi-autogenous mills used in metallurgical mines are easily affected by strong impact, abrasive wear and corrosive wear during service. In addition, the existing preparation methods of Cr-Mo steel have problems such as complex operation and difficult process control, which limits the large-scale production of Cr-Mo steel. Summary of the invention

[0004] Aiming at the problems that Cr-Mo steel liner is easy to break under the working conditions of high hardness abrasive and large impact stress, and has poor wear resistance, the present invention provides a highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill and a preparation method thereof.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention is to provide a highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill, which comprises the following chemical components by mass percentage:

[0007] C: 0.6-1.0%, Cr: 1.5-2.5%, Ti: 1.0-2.0%, Mo: 0.5-2.0%, V: 0.2-1.0%, Nb: 0.03-0.09%, Si: 1.5-2.0%, P: ≤0.003%, S: ≤0.005%, and the rest are Fe and unavoidable impurities.

[0008] Preferably, the chemical composition further includes Ti: 1.0-2.0%.

[0009] More preferably, the chemical composition is as follows, by mass percentage:

[0010] C: 0.87%, Cr: 1.58%, Mo: 0.78%, V: 0.56%, Ti: 1.0%, Nb: 0.056%, Si: 1.64%, P: 0.002%, S: 0.002%, and the rest are Fe and inevitable impurities.

[0011] The Cr-Mo steel of the present invention is composed of a microstructure composed of martensite and wear-resistant granular carbides embedded in the martensite; the wear-resistant granular carbides are one or more of TiC, Mo2C and VC, accounting for 1-5% of the area fraction of the microstructure of the Cr-Mo steel liner, and the particle size is 5-20μm.

[0012] Preferably, the highly wear-resistant Cr-Mo steel liner for the lightweight semi-autogenous mill is a hollow structure.

[0013] The weight of the hollow liner prepared in the manner of the present invention can be reduced by 20-50% compared with the solid steel liner.

[0014] The second technical solution of the present invention is to provide a method for preparing the above-mentioned highly wear-resistant Cr-Mo steel liner for a lightweight semi-autogenous mill, comprising the following steps:

[0015] (1) Smelting: adding raw materials according to mass percentage, melting, slagging, refining, and obtaining refined molten steel;

[0016] (2) Deterioration treatment: subjecting the refined molten steel to deterioration treatment to obtain deteriorated molten steel;

[0017] (3) Pouring: pouring the modified molten steel into the mold cavity at the pouring temperature, letting it stand, boxing, cleaning, and obtaining a prefabricated casting;

[0018] (4) Heat treatment: quenching and tempering the prefabricated casting, quenching the casting to room temperature to complete the quenching, and then tempering the quenched casting to obtain the highly wear-resistant Cr-Mo steel liner for the lightweight semi-autogenous mill.

[0019] Preferably, in step (1), the raw materials include scrap steel, ferroniobium, ferromolybdenum, ferrochrome and ferrovanadium; the melting is performed by heating the temperature to 1480-1580°C and then keeping the temperature for 2-5 minutes; a slag forming agent is added before slagging; and the refining is argon blowing refining.

[0020] Preferably, in step (2), the temperature of the modification treatment is 1450-1550° C.; the modification treatment uses a rare earth alloy containing niobium as a modifier, and the amount of the modifier added is 0.05-0.15% of the total mass of the refined Cr-Mo steel liquid.

[0021] Preferably, in step (3): the pouring temperature is 1400-1450°C.

[0022] Preferably, in step (4), the specific process of quenching is to heat to 800-900°C at a heating rate of 60-100°C / h, keep warm for 3-5h, and then cool to room temperature with water, the water temperature is less than 40°C; the specific process of tempering is to heat to 200-300°C at a heating rate of 60-100°C / h, keep warm for 5-6h, and then cool to room temperature under natural conditions.

[0023] The beneficial technical effects of the present invention are as follows:

[0024] The invention improves the wear resistance of the liner under high impact energy conditions and enhances the yield strength and tensile hardness of the material by controlling the wear-resistant granular carbides dispersed in the Cr-Mo steel matrix.

[0025] The present invention reduces the casting modulus of the liner, thereby reducing the microstructure defects of the thick and large cross-section to improve the casting and mechanical properties of the liner, and reduces the weight of a single liner to reduce the production cost.

[0026] The highly wear-resistant Cr-Mo steel liner for the lightweight semi-autogenous mill manufactured by the present invention has significantly improved properties such as hardness, impact toughness, and impact wear, and the liner does not deform or break during use. The manufacturing process is simple and easy to operate, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The schematic diagrams are the structural diagrams of the liner plates prepared in Example 2 and Comparative Example 1. Among them, (a) is the structural diagram of the liner plate prepared in Comparative Example 1, and (b) is the structural diagram of the liner plate prepared in Example 2.

[0028] Figure 2 The metallographic images of the thick part microstructure of the liner prepared in Example 2 and Comparative Example 1. Among them, (a) is the metallographic image of the thick part microstructure of the cross section of the liner prepared in Comparative Example 1, and (b) is the metallographic image of the thick part microstructure of the liner prepared in Example 2. DETAILED DESCRIPTION

[0029] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0030] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0031] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.

[0034] Example 1

[0035] Calculated by mass percentage, the chemical composition contents of the highly wear-resistant Cr-Mo steel liner for lightweight semi-autogenous mill are as follows:

[0036] C: 0.87%, Cr: 1.58%, Mo: 0.78%, V: 0.56%, Ti: 1.0%, Nb: 0.056%, Si: 1.64%, P: 0.002%, S: 0.002%, and the rest are Fe and inevitable impurities.

[0037] The specific preparation steps are as follows:

[0038] (1) Smelting: Smelting is carried out in an electric arc furnace. Scrap steel is first added during the smelting process. After the scrap steel is melted, ferroniobium, ferromolybdenum, ferrochrome and ferrovanadium are added in sequence. After complete melting, sampling and analysis are performed, and the composition is adjusted until it meets the mass percentage requirements of the chemical composition of the Cr-Mo steel. Slag-making agent is added, and after two slag removals, the temperature is raised to the smelting temperature of 1500°C, kept warm for 4 minutes, and then refined by blowing argon in the furnace to obtain refined steel liquid;

[0039] (2) Steel tapping and modification: The refined Cr-Mo steel liquid is poured into a ladle and treated with a niobium-containing rare earth alloy modifier at a modification temperature of 1460°C to obtain modified Cr-Mo steel liquid;

[0040] (3) Pouring, boxing and cleaning: The metamorphic Cr-Mo steel liquid is poured into a pre-prepared hollow casting mold cavity at a pouring temperature of 1420°C, and is boxed after being left to stand for 2 hours. The pouring head is then removed by an impact method, the burrs on the edges are manually cleaned, and the residual roots of the pouring head are polished to obtain a prefabricated casting;

[0041] (4) Heat treatment: After the boxed casting is loaded into a trolley furnace, it is heated to 600°C at a heating rate of 100°C / h and kept at this temperature for 4 hours. Then, it is further heated to 900°C at a heating rate of 100°C / h and kept at this temperature for 5 hours. It is then water-cooled until the liner is completely cooled. Finally, it is heated to 300°C at a heating rate of 100°C / h, kept at this temperature for 6 hours, and then air-cooled to room temperature to complete the tempering process, thereby obtaining the highly wear-resistant Cr-Mo steel liner H-1 for the lightweight semi-autogenous mill.

[0042] Example 2

[0043] Calculated by mass percentage, the chemical composition contents of the highly wear-resistant Cr-Mo steel liner for lightweight semi-autogenous mill are as follows:

[0044] C: 0.87%, Cr: 1.58%, Mo: 0.88%, Ti: 1.0%, V: 0.66%, Nb: 0.058%, Si: 1.64%, P: 0.002%, S: 0.002%, and the rest are Fe and inevitable impurities.

[0045] The specific preparation process is shown in Example 1, and the highly wear-resistant Cr-Mo steel liner H-2 for the lightweight semi-autogenous mill is prepared.

[0046] Example 3

[0047] Calculated by mass percentage, the chemical composition contents of the highly wear-resistant Cr-Mo steel liner for lightweight semi-autogenous mill are as follows:

[0048] C: 0.87%, Cr: 1.58%, Mo: 0.78%, V: 0.56%, Nb: 0.056%, Si: 1.64%, P: 0.002%, S: 0.002%, and the rest are Fe and inevitable impurities.

[0049] The specific preparation process is shown in Example 1, and the highly wear-resistant Cr-Mo steel liner H-3 for the lightweight semi-autogenous mill is prepared.

[0050] The structural diagram of H-2 is shown in Figure 1 In (b), the SEM image of the thick part of the microstructure of H-2 is shown in Figure 2 Middle (b).

[0051] Comparative Example 1

[0052] The only difference from Example 2 is that the hollow casting mold cavity in step (3) is replaced with a solid casting mold cavity to obtain the Cr-Mo steel liner S-1.

[0053] The structural diagram of S-1 is shown in Figure 1 In (a), the thick part microstructure of S-1 is shown in Figure 2 Middle (a).

[0054] Figure 2 The microstructure diagram of the thick part of the liner prepared in Example 2 and Comparative Example 1.

[0055] Among them, (a) is the microstructure diagram of the thickest part of the cross section of the lining plate prepared in Comparative Example 1, and (b) is the microstructure diagram of the thickest part of the lining plate prepared in Example 2. Figure 2 It can be seen that when the liner modulus decreases, the martensitic needles in the thick part of the liner become finer, the distribution of carbides becomes more uniform, the hole defects disappear, and the liner structure becomes denser. This shows that the present invention improves the density of the liner microstructure by changing the liner structure and reducing the casting modulus of the liner, thereby reducing the microstructure casting defects of thick and large sections.

[0056] Effect verification

[0057] (1) The Cr-Mo steel liner plates prepared in Examples 1-2 and Comparative Example 1 were used for mechanical property tests; the mechanical property tests included initial hardness, tensile strength, elongation at break, dynamic wear, carbide area fraction, and service life. The tensile strength mechanical property specimen size specifications were obtained from GB6397-86 standard; the dynamic wear test conditions were: impact energy 2J, impact frequency 100 times / min, wear time 60min; the carbide area fraction was measured by a scanning electron microscope; the service life was obtained by testing a semi-autogenous mill (specification Φ10x3.2m, cylinder speed 30r / min, filling rate 50%, daily ore processing capacity 12,000 tons). The test results are shown in Table 1.

[0058] Table 1 Mechanical properties test table

[0059]

[0060] From the comparison between H-1 and H-2 in Table 1, it can be seen that when only Mo, V, Ti are changed and the Fe ratio is adaptively adjusted, the carbide area fraction increases from 6.5% to 7.8%, the tensile strength of the Cr-Mo steel liner obtained increases from 771.6MPa to 801.1MPa, the dynamic load wear amount decreases from 0.029g to 0.021g, and the service life increases from 4442h to 4890h. The present invention improves the wear resistance of the liner under high impact energy conditions, enhances the tensile strength of the material, and increases the service life of the liner by controlling the wear-resistant granular carbides dispersed in the Cr-Mo steel matrix.

[0061] From the comparison between H-2 and S-1 in Table 1, it can be seen that although H-2 reduces the amount of raw materials, its tensile strength not only does not decrease, but increases from 654.2 to 801.1 MPa. This proves that the present invention reduces the microstructure defects of thick and large sections by reducing the casting modulus of the liner, thereby improving the casting and mechanical properties of the liner.

[0062] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a Cr-Mo steel liner for a semi-autogenous mill, It is characterized in that The following steps are involved: (1) Smelting: adding raw materials according to mass percentage, melting, slagging, refining, and obtaining refined molten steel; (2) Modification treatment: The refined molten steel is subjected to modification treatment to obtain modified molten steel; the temperature of the modification treatment is 1450-1550° C. The rare earth alloy containing niobium is used as a modifier in the modification treatment, and the amount of the modifier added is 0.05-0.15% of the total mass of the refined Cr-Mo molten steel; (3) Pouring: pouring the modified molten steel into the mold cavity at the pouring temperature, letting it stand, boxing, cleaning, and obtaining a prefabricated casting; (4) heat treatment: quenching and tempering the prefabricated casting, quenching the casting to room temperature to complete quenching, and tempering the quenched casting to obtain the Cr-Mo steel liner for the semi-autogenous mill; the specific process of the quenching is heating to 800-900°C at a heating rate of 60-100°C / h, keeping warm for 3-5h, and then cooling to room temperature with water, the water temperature is less than 40°C; the specific process of the tempering is heating to 200-300°C at a heating rate of 60-100°C / h, keeping warm for 5-6h, and then cooling to room temperature under natural conditions; The steel liner is composed of the following chemical components by mass percentage: C: 0.6-1.0%, Cr: 1.5-2.5%, Ti: 1.0-2.0%, Mo: 0.5-2.0%, V: 0.2-1.0%, Nb: 0.03-0.09%, Si: 1.5-2.0%, P: ≤0.003%, S: ≤0.005%, and the rest are Fe and unavoidable impurities; the Cr-Mo steel liner for the semi-autogenous mill is a hollow structure.

2. The method for preparing the Cr-Mo steel liner for the semi-autogenous mill according to claim 1, It is characterized in that In step (3): the pouring temperature is 1400-1450°C.

Citation Information

Patent Citations

  • Anti-fracture and anti-fatigue lining plate of semi-autogenous mill and preparation method thereof

    CN114622131A