A high-efficiency permeable perforated nonwoven fabric and preparation method thereof

By designing appropriate breathable hole structures and using specific raw materials in non-woven fabrics, the air permeability and permeability performance of non-woven fabrics are improved, the problems of insufficient air permeability and permeability performance in the existing technology are solved, and high-efficiency permeability effects are achieved. Reduced production costs.

CN115961426BActive Publication Date: 2024-10-15HANGZHOU TOMORROW FLEXIBLE PACKAGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211668789.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-24
Publication Date
2024-10-15
Estimated Expiration
2042-12-24

AI Technical Summary

Technical Problem

The air permeability and permeability of existing non-woven fabrics are not ideal and cannot meet market demand.

Method used

By controlling the diameter of the breathable holes in the non-woven fabric to 0.5-5mm, the spacing between adjacent holes is 2-4 times, the opening rate is 10-25%, using hollow fibers and multi-effect penetration microporous structures, and using 5A zeolite molecular sieves And water-soluble starch granules and other raw materials, combined with special dispersants and additives, are hot pressed and punched.

Benefits of technology

It significantly improves the air permeability and permeability of non-woven fabrics, solves the problems of poor air permeability and permeability, reduces production costs, and achieves excellent fresh-keeping performance and weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115961426B_ABST
    Figure CN115961426B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of non-woven fabric preparation, in particular to a highly efficient permeable perforated non-woven fabric and a preparation method thereof. A highly efficient permeable perforated non-woven fabric comprises a non-woven fabric body, the non-woven fabric body is provided with air holes; the diameter of the air holes is controlled at 0.5-5 mm, and the spacing between adjacent air holes is equal to 2-4 times the diameter of the air holes; the opening rate of the non-woven fabric body is equal to 10-25%. The present application has the effect of efficient penetration, solves the problems of poor air permeability and permeability in the related art, and the preparation method provided by the present application is relatively simple, the required equipment is relatively conventional, and small and medium-sized enterprises can implement it, which is convenient for market promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nonwoven fabric preparation, and in particular to a high-efficiency permeable perforated nonwoven fabric and a preparation method thereof. Background Art

[0002] At present, the non-woven fabrics used in the market are directly used, such as tea bags, sachets, seasoning bags, shoes, leather, mattresses, etc. After market research, it was found that most of the non-woven fabrics in the related art have not been processed by the punching process, and the air permeability and permeability are not ideal, which cannot meet the needs of the current market. A small number of non-woven fabrics have been processed by commercially available punching equipment to improve the air permeability and permeability, but the actual air permeability and permeability are also unsatisfactory. Therefore, the present application proposes a method for preparing a highly efficient permeable perforated non-woven fabric. Summary of the invention

[0003] In order to solve the problems existing in the above-mentioned technology, the present application provides a high-efficiency permeable perforated non-woven fabric and a preparation method thereof.

[0004] The high-efficiency permeable perforated nonwoven fabric provided in this application is realized by the following technical solutions:

[0005] A high-efficiency permeable perforated nonwoven fabric comprises a nonwoven fabric body, wherein the nonwoven fabric body is provided with air holes; the diameter of the air holes is controlled to be 0.5-5 mm, and the spacing between adjacent air holes is equal to 2-4 times of the diameter of the air holes; and the opening rate of the nonwoven fabric body is equal to 10-25%.

[0006] The high-efficiency permeable perforated nonwoven fabric prepared by the present application has the effect of high-efficiency permeability and is a nonwoven fabric product with excellent air permeability and permeability, which solves the problem of relatively poor air permeability and permeability in related technologies. The research and development team of the present application screened out the best preferred solution through the study of the opening rate and the diameter of the air holes, and the comprehensive production cost is relatively low, which meets the production needs of composite nonwoven fabric enterprises, has strong feasibility, and has the potential to be actually put on the market.

[0007] Preferably, the staple fibers constituting the main body of the nonwoven fabric are hollow fibers; the hollow fibers form a hollow cavity; the surface of the hollow fibers has multi-effect permeable micropores connected to the hollow cavity; the diameter of the hollow fibers is controlled at 20-40 microns; the wall thickness of the hollow fibers is controlled at 5-15 microns.

[0008] By adopting the above technical solution, it can be ensured that the present application has excellent air permeability and permeability.

[0009] Preferably, the non-woven fabric body is prepared from the following raw materials in percentage by mass: 8-20% of 5A zeolite molecular sieve, 2-6% of water-soluble starch particles, 0.5-2% of dispersant, 0.1-0.5% of anti-ultraviolet additive, 0.2-1% of antioxidant, and the remainder is food-grade resin granules; the food-grade resin granules are food-grade PP or PE resins; the particle size of the water-soluble starch particles is equal to 0.9-1.2 times the wall thickness of the hollow fiber (10); the particle size of the 5A zeolite molecular sieve is equal to 0.5-0.9 times the wall thickness of the hollow fiber (10).

[0010] By adopting the above technical scheme, a high-efficiency permeable perforated non-woven fabric with excellent air permeability and permeability can be prepared. And the formula components of the high-efficiency permeable perforated non-woven fabric are relatively conventional, easy to purchase in the market, highly feasible, and have the potential to be actually put on the market. In addition, the use of 5A zeolite molecular sieve in this application improves the overall air permeability and permeability, and the improvement can also improve the freshness-keeping performance of the guaranteed product. In addition, the water-soluble starch granules are conducive to the formation of multi-effect permeable micropores in the prepared hollow fibers, thereby ensuring that the present application has excellent air permeability and permeability.

[0011] Preferably, the non-woven fabric body is prepared from the following raw materials in percentage by mass: 15-18% of 5A zeolite molecular sieve, 4-5% of water-soluble starch particles, 0.5-2% of dispersant, 0.1-0.3% of anti-UV additive, 0.4-0.6% of antioxidant, and the remainder is food-grade resin granules; the food-grade resin granules are food-grade PP or PE resin; the particle size of the water-soluble starch particles is equal to 0.95-0.98 times the wall thickness of the hollow fiber; the particle size of the 5A zeolite molecular sieve is equal to 0.75-0.8 times the wall thickness of the hollow fiber.

[0012] By adopting the above technical solution, it can be further ensured that the present application has excellent air permeability and permeability, and under the premise of ensuring excellent air permeability and permeability, the overall production cost can be reduced.

[0013] Preferably, the dispersant is mainly made of KH-792 coupling agent and KH-570 coupling agent; the mass ratio of the KH-792 coupling agent and the KH-570 coupling agent is 1:(1.05-1.2); the preparation method of the dispersant comprises mixing accurately measured KH-792 coupling agent and KH-570 coupling agent uniformly, and then refluxing at 80±5°C for 2-5h to obtain a composite coupling agent, i.e., the target dispersant.

[0014] The special dispersant used in this application can perform surface treatment on water-soluble starch particles and 5A zeolite molecular sieves, so that the water-soluble starch particles and 5A zeolite molecular sieves are well compatible with the resin matrix, ensuring the improvement of the mechanical strength of the application and giving the application good air permeability and permeability.

[0015] Preferably, the anti-ultraviolet auxiliary agent is at least one of UV-326, UV-531, UV-9, and UV-320; the oxidant 1010 and the antioxidant 168; the mass ratio of the antioxidant 1010 and the antioxidant 168 is (6-8): (2-4).

[0016] By adopting the above technical solution, the present application can be endowed with good weather resistance and a relatively long service life.

[0017] The present application provides a method for preparing a highly efficient permeable perforated nonwoven fabric, which is achieved through the following technical solutions:

[0018] A method for preparing a high-efficiency permeable perforated nonwoven fabric comprises the following steps:

[0019] Step 1, drying the food-grade resin pellets for later use;

[0020] At the same time, accurately measured 5A zeolite molecular sieve, water-soluble starch granules, anti-ultraviolet additives, and antioxidants are added to the stirring kettle, stirred at a speed of 50-80 rpm, and after stirring for 5-10 minutes, the dispersant is added dropwise at a dropping amount of 2-4 mL / 10s. After the addition is completed, the mixture is stirred at a speed of 120-160 rpm for 5-20 minutes to obtain a mixture;

[0021] Step 2, high temperature melting: the food-grade resin pellets and the mixed material dried in step 1 are put into the extrusion equipment for extrusion melting, and the extruded molten material is controlled by the metering pump to extrude a specified amount according to the set requirements;

[0022] Step 3, spinning: after extrusion, the spinning solution passes through a special-shaped spinneret and is air-cooled to form hollow fibers;

[0023] Step 4: Spreading the steel mesh: The hollow fibers formed by the cooling of the special-shaped spinneret are evenly spread on the steel mesh to form a wide cloth shape;

[0024] Step 5, hot pressing: forming a wide cloth-like non-woven fabric, and then hot pressing it with a heated steel roller to press it into a thin non-woven fabric, and then cooling it after hot pressing to form a non-woven fabric;

[0025] Step 6, punching: set the temperature of the alloy steel needle at 160-200℃, and perform punching on the surface of the non-woven fabric in a rolling manner. The diameter of the air holes formed on the non-woven fabric is 0.5-5mm, and the interval between adjacent needles is 2-4 times the diameter of the needle hole; the spacing between adjacent air holes is 2-2.7 times the diameter of the air holes;

[0026] Step seven: washing, drying, rolling, and slitting into rolls of different widths to obtain finished non-woven fabrics.

[0027] The preparation method provided in this application is relatively simple, the required equipment is relatively conventional, and it can be implemented by small and medium-sized enterprises, which is convenient for market promotion and application.

[0028] Preferably, in step six, punching: setting the temperature of the punching needle at 160-200°C, punching the non-woven fabric surface in a rolling manner, the diameter of the air holes formed in the non-woven fabric is 1-3mm, and the interval between adjacent pinholes is 1.0-1.2 times the diameter of the pinhole.

[0029] By adopting the above technical solution, the air permeability and permeability performance of the present application can be further optimized.

[0030] Preferably, in step six, punching: setting the temperature of the punching needle at 160-200°C, punching the non-woven fabric surface in a rolling manner, the diameter of the air holes formed in the non-woven fabric is 1±0.05mm, and the interval between adjacent pinholes is twice the diameter of the pinhole.

[0031] By adopting the above technical solution, the air permeability and permeability performance of the present application can be further optimized.

[0032] Preferably, the method further includes step eight, wherein the finished non-woven fabric in step seven is first immersed in a 0.5-2 mol calcium chloride solution for 6-12 hours, then washed with deionized water at least twice, then immersed in a 2-4 mol sodium chloride solution, placed under 20-40 KPa, immersed for 2-8 hours, and dried to obtain a finished high-efficiency permeable perforated non-woven fabric.

[0033] By adopting the above technical solution, the air permeability and permeability performance of the present application can be further optimized.

[0034] In summary, this application has the following advantages:

[0035] 1. The present invention has the effect of efficient penetration, and solves the problem of poor air permeability and permeability in the related art.

[0036] 2. The preparation method provided in this application is relatively simple, and the required equipment is relatively conventional, and can be implemented by small and medium-sized enterprises, which is convenient for market promotion and application.

[0037] 3. The non-woven fabric body in the present application is composed of specially made hollow fibers, which can effectively ensure the air permeability and permeability of the present application, and can prepare non-woven fabric products with excellent air permeability and permeability.

[0038] 4. The special dispersant used in this application can perform surface treatment on water-soluble starch particles and 5A zeolite molecular sieve, so that the water-soluble starch particles and 5A zeolite molecular sieve are well compatible with the resin matrix, ensuring the improvement of the mechanical strength of this application and giving this application good air permeability and permeability. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram of the overall structure of the high-efficiency permeable perforated non-woven fabric in Example 1 of the present application.

[0040] Figure 2 It is a schematic diagram of the structure of the hollow fibers in the high-efficiency permeable perforated nonwoven fabric in Example 1 of the present application.

[0041] In the figure, 1. non-woven fabric body; 10. hollow fibers; 101. hollow chambers; 102. multi-effect permeable micropores; 2. air holes. DETAILED DESCRIPTION

[0042] The present application is further described in detail below in conjunction with the accompanying drawings, comparative examples and embodiments.

[0043] Example

[0044] Example 1

[0045] Reference Figure 1 , a high-efficiency permeable perforated nonwoven fabric disclosed in the present application includes a nonwoven fabric body 1, the nonwoven fabric body 1 is provided with air holes 2, the diameter of the air holes 2 is controlled to be 0.5-5mm, the spacing between adjacent air holes 2 is equal to 2-4 times the diameter of the air holes 2; the opening rate of the nonwoven fabric body 1 is equal to 10-25%. In this embodiment, the diameter of the air holes 2 is controlled to be 2mm, the spacing between adjacent air holes 2 is 3mm, and the opening rate of the nonwoven fabric body 1 is equal to 18%.

[0046] Reference Figure 1 and Figure 2 The short fibers constituting the nonwoven fabric body 1 are hollow fibers 10. The hollow fibers 10 are formed with hollow chambers 101; the surface of the hollow fibers 10 is formed with multi-effect permeable micropores 102 communicating with the hollow chambers 101. The diameter of the hollow fibers 10 is controlled to be 20-40 microns; and the wall thickness of the hollow fibers 10 is controlled to be 5-15 microns.

[0047] In this embodiment, the diameter of the hollow fiber 10 is 25±1 micrometers, and the wall thickness of the hollow fiber 10 is 8±0.5 micrometers.

[0048] The non-woven fabric body 1 is made of the following raw materials in mass percentage: 8% 5A zeolite molecular sieve, 4% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the balance is food-grade PE resin. Among them, the average particle size of the water-soluble starch particles is equal to 5-7 microns. The particle size of the 5A zeolite molecular sieve is equal to 3-5 microns.

[0049] The dispersant is mainly made of KH-792 coupling agent and KH-570 coupling agent.

[0050] The mass ratio of KH-792 coupling agent to KH-570 coupling agent is 1:1.06.

[0051] The preparation method of the dispersant is to uniformly mix accurately measured KH-792 coupling agent and KH-570 coupling agent, and reflux the mixture at 80±1° C. for 2.5 hours to obtain a composite coupling agent, i.e., the target dispersant.

[0052] The method for preparing a high-efficiency permeable perforated nonwoven fabric comprises the following steps:

[0053] Step 1: Dry the food-grade resin pellets at 90-95°C for 12 hours for later use;

[0054] Meanwhile, a dispersant was prepared by uniformly mixing accurately measured KH-792 coupling agent and KH-570 coupling agent, and then refluxed at 80±1°C for 2.5h to obtain a composite coupling agent, i.e., the target dispersant;

[0055] At the same time, accurately measured 5A zeolite molecular sieve, water-soluble starch granules, anti-ultraviolet additives, and antioxidants were added into a stirring kettle, stirred at 80 rpm, and after stirring for 5 minutes, a dispersant was added dropwise at a rate of 4 mL / 10 s. After the addition was completed, the mixture was stirred at 150 rpm for 10 minutes to obtain a mixture;

[0056] Step 2, high temperature melting: put the food-grade resin pellets and mixed materials dried in step 1 into the extrusion equipment for extrusion melting, the extrusion temperature is 150-180°C, the extruded molten material is controlled by the metering pump to extrude the specified amount according to the set requirements, and the pump supply is controlled at 32rpm;

[0057] Step 3, spinning: after extrusion, the spinning solution passes through a special-shaped spinneret and is air-cooled to form hollow fibers;

[0058] Step 4: Spreading the steel mesh: The hollow fibers formed by the cooling of the special-shaped spinneret are evenly spread on the steel mesh to form a wide cloth shape;

[0059] Step 5, hot pressing: forming a wide cloth-like non-woven fabric, and then hot pressing it with a heated steel roller to press it into a thin non-woven fabric, and then cooling it after hot pressing to form a non-woven fabric;

[0060] Step 6, punching: set the temperature of the hole needle at 180°C, and perform hole punching on the surface of the non-woven fabric in a rolling manner. The diameter of the air holes formed on the non-woven fabric is 2mm, and the interval between adjacent air holes is 3mm;

[0061] Step seven: washing, drying, rolling, and slitting into rolls of different widths to obtain finished non-woven fabrics.

[0062] Example 2

[0063] The difference between Example 2 and Example 1 is that it also includes step eight, first soaking the finished non-woven fabric in step seven in 1 mol calcium chloride solution, the mass ratio of the finished non-woven fabric to the calcium chloride solution is 1:5, soaking for 12 hours, then washing twice with deionized water, and then soaking in 2 mol sodium chloride solution, the mass ratio of the sodium chloride solution to the calcium chloride solution is 1:4, placing it under a pressure of 20 Kpa, soaking for 6 hours, and drying to obtain a finished high-efficiency permeable perforated non-woven fabric.

[0064] Example 3

[0065] The difference between Example 3 and Example 1 is that the diameter of the air holes 2 is controlled at 1 mm, the spacing between adjacent air holes 2 is 1.8 mm, and the opening rate of the non-woven fabric body 1 is equal to 18%.

[0066] Example 4

[0067] The difference between Example 4 and Example 1 is that the diameter of the air holes 2 is controlled at 3 mm, the spacing between adjacent air holes 2 is 4 mm, and the opening rate of the non-woven fabric body 1 is equal to 18%.

[0068] Example 5

[0069] The difference between Example 5 and Example 1 is that the diameter of the air holes 2 is controlled at 5 mm, the spacing between adjacent air holes 2 is 8 mm, and the opening rate of the non-woven fabric body 1 is equal to 18%.

[0070] Example 6

[0071] The difference between Example 6 and Example 1 is that the opening rate of the non-woven fabric body 1 is equal to 10%.

[0072] Example 7

[0073] The difference between Example 7 and Example 1 is that the opening rate of the non-woven fabric body 1 is equal to 25%.

[0074] Example 8

[0075] The difference between Example 8 and Example 1 is:

[0076] The nonwoven fabric body 1 is prepared from the following raw materials in percentage by mass: 15% 5A zeolite molecular sieve, 4% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0077] Example 9

[0078] The difference between Example 9 and Example 1 is:

[0079] The nonwoven fabric body 1 is prepared from the following raw materials in percentage by mass: 20% 5A zeolite molecular sieve, 4% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0080] Example 10

[0081] The difference between Example 10 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in percentage by mass: 8% 5A zeolite molecular sieve, 2% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0082] Embodiment 11

[0083] The difference between Example 11 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in the following mass percentages: 8% 5A zeolite molecular sieve, 6% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0084] Example 12

[0085] The difference between Example 12 and Example 1 is:

[0086] In this embodiment, the diameter of the air holes is controlled at 1 mm, the spacing between adjacent air holes is 1.8 mm, the porosity of the non-woven fabric body is equal to 20%, and the diameter of the hollow fiber in this embodiment is 20±1 microns, and the wall thickness of the hollow fiber 10 is 5±0.5 microns.

[0087] The non-woven fabric body 1 is made of the following raw materials in mass percentage: 16% 5A zeolite molecular sieve, 6% water-soluble starch particles, 1.8% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the balance is food-grade PE resin. Among them, the average particle size of the water-soluble starch particles is equal to 4-5 microns. The particle size of the 5A zeolite molecular sieve is equal to 2-4 microns.

[0088] The dispersant is mainly made of KH-792 coupling agent and KH-570 coupling agent.

[0089] The mass ratio of KH-792 coupling agent to KH-570 coupling agent is 1:1.08.

[0090] The preparation method of the dispersant is to uniformly mix accurately measured KH-792 coupling agent and KH-570 coupling agent, and reflux the mixture at 80±1° C. for 3 hours to obtain a composite coupling agent, namely, the target dispersant.

[0091] The method for preparing a high-efficiency permeable perforated nonwoven fabric comprises the following steps:

[0092] Step 1: Dry the food-grade resin pellets at 90-95°C for 12 hours for later use;

[0093] Meanwhile, a dispersant was prepared by uniformly mixing accurately measured KH-792 coupling agent and KH-570 coupling agent, and then refluxed at 80±1°C for 3h to obtain a composite coupling agent, i.e., the target dispersant;

[0094] At the same time, accurately measured 5A zeolite molecular sieve, water-soluble starch granules, anti-ultraviolet additives, and antioxidants were added into a stirring kettle, stirred at 80 rpm, and after stirring for 10 min, a dispersant was added dropwise at a rate of 4 mL / 10 s. After the addition was completed, the mixture was stirred at 150 rpm for 20 min to obtain a mixture;

[0095] Step 2, high temperature melting: put the food-grade resin pellets and mixed materials dried in step 1 into the extrusion equipment for extrusion melting, the extrusion temperature is 150-180°C, the extruded molten material is controlled by the metering pump to extrude the specified amount according to the set requirements, and the pump supply is controlled at 28rpm;

[0096] Step 3, spinning: after extrusion, the spinning solution passes through a special-shaped spinneret and is air-cooled to form hollow fibers;

[0097] Step 4: Spreading the steel mesh: The hollow fibers formed by the cooling of the special-shaped spinneret are evenly spread on the steel mesh to form a wide cloth shape;

[0098] Step 5, hot pressing: forming a wide cloth-like non-woven fabric, and then hot pressing it with a heated steel roller to press it into a thin non-woven fabric, and then cooling it after hot pressing to form a non-woven fabric;

[0099] Step 6, punching: set the temperature of the hole needle at 200°C, and perform a punching process on the surface of the non-woven fabric in a rolling manner. The diameter of the air holes formed on the non-woven fabric is 1mm, and the interval between adjacent air holes is 1.8mm;

[0100] Step seven, washing, drying, rolling, and slitting into rolls of different widths to obtain finished non-woven fabrics;

[0101] Step eight, soak the finished non-woven fabric in step seven in a 1.2 mol calcium chloride solution, the mass ratio of the finished non-woven fabric to the calcium chloride solution is 1:4, soak for 12 hours, then wash twice with deionized water, and then soak in a 2 mol sodium chloride solution, the mass ratio of the sodium chloride solution to the calcium chloride solution is 1:4, place it under a pressure of 20 Kpa, soak for 8 hours, and dry it to obtain a finished high-efficiency permeable perforated non-woven fabric.

[0102] Comparative Example

[0103] Comparative Example 1

[0104] The difference between Comparative Example 1 and Example 1 is that the diameter of the air holes 2 is controlled at 8 mm, the spacing between adjacent air holes 2 is 16 mm, and the opening rate of the non-woven fabric body 1 is equal to 18%.

[0105] Comparative Example 2

[0106] The difference between Comparative Example 2 and Example 1 is that the diameter of the air holes 2 is controlled at 8 mm, the spacing between adjacent air holes 2 is 16 mm, and the opening rate of the non-woven fabric body 1 is equal to 30%.

[0107] Comparative Example 3

[0108] The difference between Comparative Example 3 and Example 1 is that the diameter of the air holes 2 is controlled at 2 mm, the spacing between adjacent air holes 2 is 3 mm, and the opening rate of the non-woven fabric body 1 is equal to 8%.

[0109] Comparative Example 4

[0110] The difference between Comparative Example 4 and Example 1 is that the diameter of the air holes 2 is controlled at 2 mm, the spacing between adjacent air holes 2 is 3 mm, and the opening rate of the non-woven fabric body 1 is equal to 30%.

[0111] Comparative Example 5

[0112] The difference between Comparative Example 5 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in percentage by mass: 5% 5A zeolite molecular sieve, 4% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0113] Comparative Example 6

[0114] The difference between Comparative Example 6 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in the following mass percentages: 25% 5A zeolite molecular sieve, 4% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0115] Comparative Example 7

[0116] The difference between Comparative Example 7 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in the following mass percentages: 8% 5A zeolite molecular sieve, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0117] Comparative Example 8

[0118] The difference between Comparative Example 8 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in percentage by mass: 8% 5A zeolite molecular sieve, 1% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0119] Comparative Example 9

[0120] The difference between Comparative Example 9 and Example 1 is that the non-woven fabric body 1 is prepared from the following raw materials in the following mass percentages: 8% 5A zeolite molecular sieve, 8% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin.

[0121] Comparative Example 10

[0122] The difference between Comparative Example 10 and Example 1 is:

[0123] The method for preparing a high-efficiency permeable perforated nonwoven fabric comprises the following steps:

[0124] Step 1: Dry the food-grade resin pellets at 90-95°C for 12 hours for later use;

[0125] Meanwhile, a dispersant was prepared by uniformly mixing accurately measured KH-792 coupling agent and KH-570 coupling agent, and then refluxed at 80±1°C for 2.5h to obtain a composite coupling agent, i.e., the target dispersant;

[0126] At the same time, accurately measured 5A zeolite molecular sieve, water-soluble starch granules, anti-ultraviolet additives, and antioxidants were added into a stirring kettle, stirred at 80 rpm, and after stirring for 5 minutes, a dispersant was added dropwise at a rate of 4 mL / 10 s. After the addition was completed, the mixture was stirred at 150 rpm for 10 minutes to obtain a mixture;

[0127] Step 2, high temperature melting: put the food-grade resin pellets and mixed materials dried in step 1 into the extrusion equipment for extrusion melting, the extrusion temperature is 150-180°C, the extruded molten material is controlled by the metering pump to extrude the specified amount according to the set requirements, and the pump supply is controlled at 32rpm;

[0128] Step 3, spinning: after extrusion, the spinning solution passes through a special-shaped spinneret and is air-cooled to form hollow fibers;

[0129] Step 4: Spreading the steel mesh: The hollow fibers formed by the cooling of the special-shaped spinneret are evenly spread on the steel mesh to form a wide cloth shape;

[0130] Step 5, hot pressing: forming a wide cloth-like non-woven fabric, and then hot pressing it through a heated steel roller to press it into a thin non-woven fabric. After hot pressing, it is cooled to form a non-woven fabric, rolled up, and cut into rolls of different widths to obtain the finished non-woven fabric.

[0131] Comparative Example 11

[0132] The difference between Comparative Example 11 and Example 1 is:

[0133] The non-woven fabric body 1 is prepared from the following raw materials in mass percentage: 8% 5A zeolite molecular sieve, 4% water-soluble starch particles, 1.5% dispersant, 0.2% anti-ultraviolet additive UV-326, 0.4% antioxidant 1010, 0.1% antioxidant 168, and the remainder is food-grade PE resin. The dispersant is KH-792 coupling agent.

[0134] The method for preparing a high-efficiency permeable perforated nonwoven fabric comprises the following steps:

[0135] Step 1: Dry the food-grade resin pellets at 90-95°C for 12 hours for later use;

[0136] At the same time, accurately measured 5A zeolite molecular sieve, water-soluble starch granules, anti-ultraviolet additives, and antioxidants were added into a stirring kettle, stirred at 80 rpm, and after stirring for 5 min, KH-792 coupling agent was added dropwise at a rate of 4 mL / 10 s. After the addition was completed, the mixture was stirred at 150 rpm for 10 min to obtain a mixture;

[0137] Step 2, high temperature melting: put the food-grade resin pellets and mixed materials dried in step 1 into the extrusion equipment for extrusion melting, the extrusion temperature is 150-180°C, the extruded molten material is controlled by the metering pump to extrude the specified amount according to the set requirements, and the pump supply is controlled at 32rpm;

[0138] Step 3, spinning: after extrusion, the spinning solution passes through a special-shaped spinneret and is air-cooled to form hollow fibers;

[0139] Step 4: Spreading the steel mesh: The hollow fibers formed by the cooling of the special-shaped spinneret are evenly spread on the steel mesh to form a wide cloth shape;

[0140] Step 5, hot pressing: forming a wide cloth-like non-woven fabric, and then hot pressing it with a heated steel roller to press it into a thin non-woven fabric, and then cooling it after hot pressing to form a non-woven fabric;

[0141] Step 6, punching: set the temperature of the hole needle at 180°C, and perform hole punching on the surface of the non-woven fabric in a rolling manner. The diameter of the air holes formed on the non-woven fabric is 2mm, and the interval between adjacent air holes is 3mm;

[0142] Step seven: washing, drying, rolling, and slitting into rolls of different widths to obtain finished non-woven fabrics.

[0143] Comparative Example 12

[0144] The difference between Comparative Example 12 and Example 11 is that the coupling agent KH-792 is replaced by conventional KH550.

[0145] Performance testing

[0146] Detection method / test method

[0147] 1. Tensile strength test: According to GB / T 24218.3-2010 Textile nonwoven fabric test methods Part 3: Determination of breaking strength and breaking elongation (strip method) of the effective permeable perforated nonwoven fabrics in Examples 1-12 and Comparative Examples 1-12. Testing instrument: electronic tensile testing machine; Electronic tensile testing machine debugging: measuring speed: 100mm / min; test width: 50mm; test gauge length: 200mm.

[0148] 2. Heat seal strength test is carried out in accordance with QB / T 2358-1998 "Test Method for Heat Seal Strength of Plastic Film Packaging Bags". Heat seal conditions: 140℃-170℃, 3 seconds, 0.3MPa, testing equipment: HST-H3 heat seal tester.

[0149] 3. The non-woven fabrics in Examples 1-12 and Comparative Examples 1-12 were made into spice bags with a size of 50 mm*50 mm. 2 g of five-spice seasoning was put into the spice bags, and the bags were boiled in water at 100°C. The time T (min) to smell the fragrance was detected.

[0150] Data analysis

[0151] Table 1 is the test parameters of Examples 1-12 and Comparative Examples 1-12

[0152]

[0153] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that by comparing Example 1 with Comparative Example 10, the present application has the effect of efficient penetration, and solves the problems of poor air permeability and permeability in the related art.

[0154] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that, compared with Example 1 and Example 2, although the tensile strength and heat seal strength of the present application have decreased after the treatment of step eight, the air permeability and permeability have improved and enhanced, and the tensile strength MD of Example 2 is ≥20N / 15mm; TD ≥7N / 15mm, and the heat seal strength is ≥16N / 15mm, which meets the national testing standards. Therefore, the non-woven fabric prepared in the present application can improve the overall air permeability and permeability after the treatment of step eight.

[0155] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that by comparing Examples 1 and 3-5 with Comparative Examples 1-2, the diameter of the air holes is controlled at 0.5-5 mm, and the spacing between adjacent air holes is equal to 0.8-4 times the diameter of the air holes. The prepared high-efficiency permeable perforated non-woven fabric has good air permeability and permeability, and has good mechanical strength and heat sealing strength, which meets national testing standards.

[0156] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that, compared with Comparative Examples 3-4, Examples 1 and 6-7 have a slightly lower mechanical strength than Comparative Example 3, but the air permeability and permeability of Examples 1 and 6-7 are better than Comparative Example 3, and the heat sealing strength of the two is similar; the mechanical strength of Examples 1 and 6-7 is greater than that of Comparative Example 4, and the air permeability and permeability of Example 7 are similar to those of Comparative Example 4. Therefore, it is appropriate to control the opening rate of the non-woven fabric body to 10-25%.

[0157] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that, compared with Comparative Examples 5-6, Examples 1 and 8-9 show that, as the zeolite content increases, the air permeability and permeability are improved, but the strength and heat seal strength decrease, but the strength and heat seal strength still meet the national testing standards. The strength and heat seal strength of Examples 1 and 8-9 are lower than those of Comparative Example 5, but the air permeability and permeability of Examples 1 and 8-9 are better than those of Comparative Example 5, and Example 9 is similar to Comparative Example 6 in terms of air permeability and permeability. Considering the cost comprehensively, the addition amount of 5A zeolite molecular sieve is preferably controlled at 10-25, and the addition amount of 5A zeolite molecular sieve is controlled at 18-20% in the best solution.

[0158] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that, by comparing Examples 1 and 10-11 with Comparative Examples 8-9, as the amount of starch added increases, the air permeability and permeability of the prepared non-woven fabric are improved. However, when the content of water-soluble starch particles exceeds 6%, although the air permeability and permeability of the non-woven fabric are improved, the overall mechanical strength is significantly reduced. Therefore, the content of water-soluble starch particles is 2-6%, and the best solution is that the content of water-soluble starch particles is 4-5%.

[0159] Combining Examples 1-12 and Comparative Examples 1-12 and Table 1, it can be seen that by comparing Example 1 with Comparative Examples 11-12, the mechanical strength and heat sealing strength of Comparative Examples 11-12 have both decreased significantly. Conventional coupling agents cannot be used to perform good surface treatment on 5A zeolite molecular sieves and water-soluble starch granules. The compatibility of 5A zeolite molecular sieves and water-soluble starch granules with the matrix resin is poor, resulting in a decrease in the overall mechanical strength and heat sealing strength. Therefore, the composite coupling agent provided in the present application can make the 5A zeolite molecular sieve and water-soluble starch granules uniformly dispersed in the matrix resin and have good compatibility with the matrix resin, thereby ensuring the overall mechanical strength and heat sealing strength of the present application, while having good air permeability and permeability.

[0160] In summary, the high-efficiency permeable perforated nonwoven fabric prepared by the present application has the effect of high-efficiency penetration, and is a nonwoven fabric product with excellent air permeability and permeability, which solves the problem of relatively poor air permeability and permeability in the related technology. Through the research on the opening rate and the diameter of the air holes, the research and development team of the present application screened out the best preferred solution, which is the technical solution of Example 12, and the comprehensive production cost is relatively low. The production needs of composite nonwoven fabric enterprises are strong, and there is potential for actual market launch.

[0161] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A highly efficient permeable perforated nonwoven fabric, characterized in that: It comprises a non-woven fabric body (1), the non-woven fabric body (1) is provided with air holes (2); the diameter of the air holes (2) is controlled to be 1 mm, and the spacing between adjacent air holes (2) is 1.8 mm; the opening rate of the non-woven fabric body (1) is equal to 20%; The staple fibers constituting the nonwoven fabric body (1) are hollow fibers (10); the hollow fibers (10) form a hollow cavity (101); the surface of the hollow fibers (10) is formed with multi-effect permeable micropores (102) communicating with the hollow cavity (101); the diameter of the hollow fibers (10) is 20±1 micrometers; the wall thickness of the hollow fibers (10) is 5±0.5 micrometers; The non-woven fabric body (1) is prepared from the following raw materials in percentage by mass: 16% of 5A zeolite molecular sieve, 6% of water-soluble starch particles, 1.8% of dispersant, 0.2% of anti-ultraviolet additive UV-326, 0.4% of antioxidant 1010, 0.1% of antioxidant 168, and the balance is food-grade PE resin, wherein the average particle size of the water-soluble starch particles is equal to 4-5 microns, and the particle size of the 5A zeolite molecular sieve is equal to 2-4 microns; The dispersant is a composite coupling agent made of KH-792 coupling agent and KH-570 coupling agent; The mass ratio of KH-792 coupling agent to KH-570 coupling agent is 1:1.08; The method for preparing a high-efficiency permeable perforated nonwoven fabric comprises the following steps: Step 1: Dry the food-grade resin pellets at 90-95°C for 12 hours for later use; Meanwhile, a dispersant was prepared by uniformly mixing accurately measured KH-792 coupling agent and KH-570 coupling agent, and then refluxed at 80±1°C for 3h to obtain a composite coupling agent, i.e., the target dispersant; At the same time, accurately measured 5A zeolite molecular sieve, water-soluble starch granules, anti-ultraviolet additives, and antioxidants were added into a stirring kettle, stirred at 80 rpm, and after stirring for 10 min, a dispersant was added dropwise at a rate of 4 mL / 10 s. After the addition was completed, the mixture was stirred at 150 rpm for 20 min to obtain a mixture; Step 2, high temperature melting: put the food-grade resin pellets and mixed materials dried in step 1 into the extrusion equipment for extrusion melting, the extrusion temperature is 150-180°C, the extruded molten material is controlled by the metering pump to extrude the specified amount according to the set requirements, and the pump supply is controlled at 28rpm; Step 3, spinning: after extrusion, the spinning solution passes through a special-shaped spinneret and is air-cooled to form hollow fibers; Step 4: Spreading the steel mesh: The hollow fibers formed by the cooling of the special-shaped spinneret are evenly spread on the steel mesh to form a wide cloth shape; Step 5, hot pressing: forming a wide cloth-like non-woven fabric, and then hot pressing it with a heated steel roller, and then cooling it to form a non-woven fabric; Step 6, punching: set the temperature of the hole needle at 200°C, and perform a punching process on the surface of the non-woven fabric in a rolling manner. The diameter of the air holes formed on the non-woven fabric is 1mm, and the interval between adjacent air holes is 1.8mm; Step seven, washing, drying, rolling, and slitting into rolls of different widths to obtain finished non-woven fabrics; Step eight, soak the finished non-woven fabric in step seven in 1.2 mol calcium chloride solution, the mass ratio of the finished non-woven fabric to the calcium chloride solution is 1:4, soak for 12 hours, then wash twice with deionized water, and then soak in 2 mol sodium chloride solution, the mass ratio of sodium chloride solution to calcium chloride solution is 1:4, place it under a pressure of 20 Kpa, soak for 8 hours, and dry it to obtain a finished high-efficiency permeable perforated non-woven fabric.