A pressure-sensitive adhesive for TPU car cover with wide temperature range and resistance to alternating hot and cold and preparation method thereof

By using a special pressure-sensitive adhesive that is resistant to alternating hot and cold and wide temperature range on TPU car clothing, combined with the formula and process steps of soft and hard monomers and acrylic rubber, the adhesion of TPU car clothing in high and low temperatures and marine climates is solved. Solve the problem of bonding performance and achieve high initial adhesion, peel strength and stability.

CN115975555BActive Publication Date: 2024-10-11XIAN AEROSPACE SUNVALOR CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210764163.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-29
Publication Date
2024-10-11
Estimated Expiration
2042-06-29

AI Technical Summary

Technical Problem

When TPU car clothing is used in high and low temperature environments and marine climate conditions, it is difficult for conventional adhesives to maintain good bonding performance, which can easily lead to the paint protective film degumming and affect the use effect.

Method used

A pressure-sensitive adhesive for TPU car clothing that is resistant to alternating hot and cold temperatures and is used in a wide temperature range. The formula includes soft monomers, hard monomers, functional monomers, solvents and acrylate rubber. Through specific weight ratios and process steps (such as heating Reflux reaction and dropping reaction), add acrylate rubber AR840 to broaden the molecular weight distribution, improve the cohesion and wetting properties of the adhesive, and add curing agent and organic solvent to the glue to enhance the cross-linking effect.

Benefits of technology

It achieves high initial adhesion, peel strength and high cohesion performance of TPU car clothing in low and high temperature environments, ensuring that no glue will fall off or remain in a wide temperature range, and its performance is stable under hot and cold cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003721680950000051
    Figure BDA0003721680950000051
  • Figure BDA0003721680950000061
    Figure BDA0003721680950000061
  • Figure BDA0003721680950000072
    Figure BDA0003721680950000072
Patent Text Reader

Abstract

The present invention discloses a TPU car cover pressure-sensitive adhesive for resistant cold and hot alternating wide temperature range, and the raw materials for preparation include by weight: 10-30 parts of soft monomer, 7-13 parts of hard monomer, 0.1-3 parts of functional monomer, 70 parts of solvent, 0.01-0.05 parts of initiator, and 0.5-3 parts of acrylate rubber. The present invention uses butyl acrylate as a soft monomer, methyl methacrylate as a hard monomer, and acrylic acid as a functional monomer to adjust the molecular weight and molecular weight distribution of the pressure-sensitive adhesive, improve the viscoelasticity and wettability of the pressure-sensitive adhesive, and obtain an adhesive with strong bonding with the TPU substrate, which is not easy to fall off when used at low temperature and room temperature. And by introducing acrylate rubber AR840, the molecular weight distribution of the pressure-sensitive adhesive is increased, the heat resistance of the pressure-sensitive adhesive is improved, the use temperature range of the pressure-sensitive adhesive is further broadened, and the high temperature and high humidity resistance of the pressure-sensitive adhesive is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a TPU pressure-sensitive adhesive for car covers that is resistant to alternating hot and cold temperatures over a wide temperature range and a preparation method thereof, and relates to C09J151 / 00, and in particular to the field of adhesives. Background Art

[0002] Car cover is a protective film that is attached to the surface of car paint using polymer materials to protect the original paint and decorate the car body. It can be easily removed at any time. It mainly includes paint protection films made of PVC, TPH and TPU. Paint protection films made of TPU have high tension, pulling force, excellent aging resistance, corrosion resistance and other characteristics, which have made it occupy the high-end product market of car paint protection films for a long time and have long-term development potential. However, the surface energy of TPU materials is low, and it is difficult to achieve good adhesion using conventional adhesives, which can easily cause the paint protection film to debond, and seriously damage the car paint and affect the use effect. In addition, the paint protection film is an external film, and the high temperature environment and low temperature environment have different forces on the paint protection film adhesive. The marine climate environment will also affect the service life of the paint protection film adhesive. Therefore, it is very important to develop a paint protection film adhesive that has wide applicability and can withstand a wide temperature range of alternating hot and cold.

[0003] Chinese invention patent CN201910097724.5 discloses a hot and cold alternating removable acrylic pressure-sensitive adhesive, a preparation method and its application. By adopting a combination of soft and hard monomer cross-linking and introducing an anionic emulsifier, a hot and cold alternating pressure-sensitive adhesive is prepared, and it has good removable performance, but the aqueous solution system has poor bonding effect with TPU substrate. Chinese invention patent CN201010521734.6 discloses a preparation method of a high-strength heat-resistant silicone resin modified acrylate pressure-sensitive adhesive. By using silicone resin to modify the acrylic pressure-sensitive adhesive, the high temperature resistance of the acrylic pressure-sensitive adhesive is improved, so that it still has good peel strength in a high temperature environment, but it is easy to become brittle in a low temperature environment, and the use effect is greatly reduced. Summary of the invention

[0004] In order to improve the performance of TPU pressure-sensitive adhesive for car cover in high and low temperature environments and increase the bonding performance between the pressure-sensitive adhesive and the TPU substrate, the first aspect of the present invention provides a pressure-sensitive adhesive for TPU car cover that is resistant to alternating hot and cold temperatures and has a wide temperature range. The raw materials for preparation include, by weight: 10-30 parts of soft monomers, 7-13 parts of hard monomers, 0.1-3 parts of functional monomers, 70 parts of solvents, 0.01-0.05 parts of initiators, and 0.5-3 parts of acrylic rubber.

[0005] As a preferred embodiment, the raw materials for preparation include, by weight: 13-24 parts of soft monomer, 7-8.5 parts of hard monomer, 0.6-1.6 parts of functional monomer, 70 parts of solvent, 0.01-0.05 parts of initiator, and 1.2-2.4 parts of acrylic rubber.

[0006] As a preferred embodiment, the soft monomer is selected from one or a combination of ethyl acrylate, butyl acrylate, isooctyl acrylate, lauryl acrylate, and 2-ethylhexyl acrylate.

[0007] As a preferred embodiment, the soft monomer is butyl acrylate.

[0008] As a preferred embodiment, the hard monomer is selected from one or a combination of methyl acrylate, methyl methacrylate, vinyl acetate, acrylonitrile, acrylamide, and styrene.

[0009] As a preferred embodiment, the hard monomer is methyl methacrylate.

[0010] As a preferred embodiment, the functional monomer is selected from one or a combination of acrylic acid, β-acryloxypropionic acid, methacrylic acid, and acrylamide.

[0011] As a preferred embodiment, the functional monomer is acrylic acid.

[0012] As a preferred embodiment, the solvent is selected from one or a combination of dimethyl carbonate, ethyl acetate, toluene, heptane, methyl acetate, n-propyl acetate, octane and hexane.

[0013] As a preferred embodiment, the solvent is a combination of dimethyl carbonate and ethyl acetate.

[0014] As a preferred embodiment, the weight ratio of dimethyl carbonate to ethyl acetate is (1-10):3.

[0015] As a preferred embodiment, the weight ratio of dimethyl carbonate to ethyl acetate is 5:3.

[0016] The applicant found during the experiment that using a combination of dimethyl carbonate and ethyl acetate as a solvent can improve the mixed dissolution effect between the various raw materials, increase the transparency of the pressure-sensitive adhesive for car covers, and reduce the impact of the pressure-sensitive adhesive on the appearance of the car cover.

[0017] As a preferred embodiment, the initiator is selected from one or a combination of organic peroxide initiators, inorganic peroxide initiators, and azo initiators.

[0018] As a preferred embodiment, the organic peroxide initiator is selected from one or a combination of benzoyl peroxide, dilauroyl peroxide, cumene hydroperoxide, tert-butyl perbenzoate, and tert-amyl peroxide 2-ethylhexanoate.

[0019] As a preferred embodiment, the initiator is an azo initiator, which is azobisisobutyronitrile.

[0020] As a preferred embodiment, the acrylic rubber is selected from one or a combination of AR74 of Japan Zeon Co., Ltd., AR840 of Japan Toa Paint Co., Ltd., AR100 of Sichuan Suining Qinglong Acrylic Rubber Factory, and AR96 of Chongqing Jianfeng Co., Ltd.

[0021] As a preferred embodiment, the acrylic rubber is AR840 produced by Japan Toa Paint Co., Ltd.

[0022] During the experiment, the applicant found that the introduction of acrylate rubber AR840 into the adhesive system broadened the molecular weight distribution range of the overall resin, allowing it to be used normally within a wider temperature range, and the amount of acrylate rubber added was 0.53-2.75% of the overall mass. On the basis of maintaining the high permeability of the adhesive, the adhesive also had a higher cohesive force, and the adhesive was not prone to falling off. The possible reasons are speculated to be: acrylate rubber AR840 is a high molecular weight resin with hard monomers as the main monomers, and its heat resistance is good. In combination with butyl acrylate and acrylic acid in this application, it has a lower glass transition temperature and achieves better low-temperature resistance. The applicant further found that the introduction of acrylate rubber AR840 with a mass fraction of 0.53-2.75% caused the adhesive to become turbid, allowing it to maintain high permeability and reducing the transparency impact caused by poor solubility. In addition, the low amount of acrylate rubber added will not destroy the cross-linked structure of the pressure-sensitive adhesive body, and can maintain a higher cohesive force of the adhesive. At the same time, due to the high modulus of acrylic rubber, it can be well dispersed in the pressure-sensitive adhesive system at a mass fraction of 0.53-2.75%, forming an effective action point on the substrate, and dispersing the interface damage between the adhesive layer and the test steel plate caused by stretching during the peeling process, ensuring that the peeling strength will not decrease but will increase. At the same time, due to the widening of the molecular weight distribution, the rapid wetting performance of the pressure-sensitive adhesive is increased, ensuring that the initial adhesion will not decrease but will increase.

[0023] The second aspect of the present invention provides a method for preparing a TPU pressure-sensitive adhesive for car covers that is resistant to alternating hot and cold temperatures over a wide temperature range, comprising the following steps:

[0024] (1) After uniformly mixing the soft monomer, hard monomer, functional monomer, solvent, initiator, and acrylic rubber according to a certain proportion, a reactant A is obtained, and the reactant A is evenly divided into two parts;

[0025] (2) adding a portion of the mixture into a reaction flask and heating the mixture to reflux the mixture, maintaining the reaction at 80-90° C. for 30-90 minutes to obtain reactant B;

[0026] (3) Then, another portion of reactant A is added dropwise to reactant B obtained in step 2 for 60-180 minutes. After the addition is completed, the temperature is kept at 80-90° C. for 3-5 hours, then cooled to room temperature, and stirred evenly after cooling to obtain the product.

[0027] The third aspect of the present invention provides a method for using a TPU pressure-sensitive adhesive for car covers that is resistant to alternating hot and cold temperatures over a wide temperature range, comprising the following steps: adding a curing agent and an organic solvent to the pressure-sensitive adhesive and stirring evenly, coating it on a TPU film with a coating machine, and obtaining the product after curing.

[0028] As a preferred embodiment, the cross-linking agent is used in an amount of 0.5-5 wt % of the weight of the pressure-sensitive adhesive.

[0029] As a preferred embodiment, the cross-linking agent is selected from one or a combination of isocyanate curing agents, aziridine curing agents, and metal salt curing agents.

[0030] More preferably, the cross-linking agent is a metal salt curing agent.

[0031] As a preferred implementation, the weight ratio of the organic solvent to the pressure-sensitive adhesive is (0.8-2):1.

[0032] As a preferred implementation, the weight ratio of the organic solvent to the pressure-sensitive adhesive is 1:1.

[0033] As a preferred embodiment, the organic solvent is ethyl acetate.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The TPU pressure-sensitive adhesive for car covers with wide temperature range and resistance to alternating cold and heat is prepared by using butyl acrylate as a soft monomer, methyl methacrylate as a hard monomer, and acrylic acid as a functional monomer. The weight ratio of the soft and hard monomers is (15-20): (7-13), and the molecular weight and molecular weight distribution of the pressure-sensitive adhesive are adjusted to improve the viscoelasticity and wettability of the pressure-sensitive adhesive, thereby obtaining an adhesive with strong bonding with the TPU substrate, which is not easy to fall off when used at low temperature or room temperature.

[0036] (2) The TPU pressure-sensitive adhesive for car covers with wide temperature range and resistance to alternating cold and heat described in the present invention increases the molecular weight distribution of the pressure-sensitive adhesive, improves the heat resistance of the pressure-sensitive adhesive, further broadens the use temperature range of the pressure-sensitive adhesive, and improves the high temperature and high humidity resistance of the pressure-sensitive adhesive.

[0037] (3) The TPU pressure-sensitive adhesive for car covers with wide temperature range and resistant to alternating heat and cold has the advantages of high initial adhesion, high peeling and high cohesion. By widening the molecular weight distribution, adding high temperature resistant resin and synergistic cross-linking, the prepared adhesive has a peeling strength of more than 1800gf / 25mm, and the adhesive retention performance reaches 150°C for 24 hours without displacement. Moreover, after 100 cycles of hot and cold cycles at -40°C without humidity (5 hours) to 65°C 50% RH (5 hours), the pressure-sensitive adhesive still has stable performance without falling off or residual adhesive. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is the infrared spectrum of the pressure-sensitive adhesive for TPU car cover in Example 1;

[0039] Figure 2 This is the thermal weight loss diagram of the pressure-sensitive adhesive for TPU car cover in Example 1;

[0040] Figure 3 This is the thermal DSC graph of the pressure-sensitive adhesive for TPU car cover in Example 1. DETAILED DESCRIPTION

[0041] Examples 1-6, Comparative Examples 1-3

[0042] A TPU pressure-sensitive adhesive for car cover with wide temperature range and resistant to alternating cold and hot conditions, the raw material formula composition of which is shown in Table 1 below, the solvent is dimethyl carbonate and ethyl acetate, the weight ratio of which is 5:3; the initiator is azobisisobutyronitrile; the acrylic rubber is AR840, purchased from Japan Toa Paint Co., Ltd. The raw materials for preparation are calculated by weight, as follows:

[0043] Table 1

[0044]

[0045] A method for preparing a TPU pressure-sensitive adhesive for car covers that is resistant to alternating hot and cold temperatures over a wide temperature range, comprising the following steps:

[0046] (1) After uniformly mixing the soft monomer, hard monomer, functional monomer, solvent, initiator, and acrylic rubber according to a certain proportion, a reactant A is obtained, and the reactant A is evenly divided into two parts;

[0047] (2) adding a portion of the mixture into a reaction flask and heating the mixture to reflux the mixture. The reaction was maintained at 84° C. for 60 minutes to obtain reactant B.

[0048] (3) Then, another portion of reactant A is added dropwise to reactant B obtained in step 2 for 120 minutes. After the addition is completed, the temperature is kept at 84° C. for 4 hours, then cooled to 25° C., and stirred evenly after cooling to obtain the product.

[0049] A method for using a TPU car cover pressure-sensitive adhesive that is resistant to alternating hot and cold temperatures over a wide temperature range comprises adding a curing agent and a solvent into the pressure-sensitive adhesive and stirring the mixture evenly, and coating the mixture on a TPU film using a coating machine.

[0050] The curing agent is an ethyl acetate solution of aluminum acetylacetonate, with a mass concentration of 5%;

[0051] The solvent is ethyl acetate;

[0052] The amount of the curing agent used is 2wt% of the weight of the pressure-sensitive adhesive, and the weight ratio of the solvent to the adhesive is 1:1.

[0053] The performance of the pressure-sensitive adhesives prepared in Examples 1-6 and Comparative Examples 1-3 was tested:

[0054] The main performance indicators of pressure-sensitive adhesive are as follows:

[0055]

[0056]

[0057] 1. Test of bonding strength with TPU: dilute the pressure-sensitive adhesive to 20% solid content with ethyl acetate, add the measured cross-linking agent and stir evenly to obtain a coating liquid; use an applicator to evenly apply it on a 25μm PET release film, dry it at 120°C for 3 minutes, and then transfer it to a 150μm TPU film to obtain a tape with a dry adhesive thickness of 25μm. After placing the sample for 24 hours, test its bonding performance with TPU according to GB / T 2792-1998 (machine pulling test), hand tearing or hand rubbing. If the adhesive does not fall off and is consistent with the original sample, it is considered qualified, indicated by ★★★★★, and the fewer ★s, the worse the test result.

[0058] 2. Glass transition temperature (Tg) test: The film prepared in Example 1 was tested by differential scanning calorimetry under the protection of N2, with a temperature range of -80 to 100°C and a heating rate of 10°C / min. The test results are shown in Figure 3 .

[0059] 3. Molecular weight and molecular weight distribution test: The membrane prepared in Example 1 was soaked in THF for a certain period of time to dissolve, and the sample was ensured to be between 3 and 4 mg. The test results are shown in Figure 1-2 .

[0060] 4. Initial adhesion test: The test method is in accordance with GB / T 2794-2013.

[0061] 5. Peel strength test: The test method refers to PSTC-101.

[0062] 6. Adhesion performance: Determined by referring to PSTC-107 method. Dilute the pressure-sensitive adhesive to 20% solid content with ethyl acetate, add the measured cross-linking agent and stir evenly to obtain a coating solution; use an applicator to evenly apply it to a 25μm PET release film, dry it at 120±5℃ for 3min, and then transfer it to a 150μm TPU film to obtain an adhesive tape with a dry adhesive thickness of 25μm. Stick the pressure-sensitive adhesive on a test piece with a width of about 200mm and a length of about 300mm and a weight of 1kg, and measure the displacement after 4 hours at 150℃ and record it.

[0063] The experimental results of Examples 1-6 are recorded in Table 2 below, and the experimental results of Comparative Examples 1-3 are recorded in Table 3 below.

[0064] Table 2

[0065]

[0066]

[0067] Table 3

[0068]

[0069] Examples 7-12, Comparative Examples 4-5

[0070] A TPU pressure-sensitive adhesive for car cover with wide temperature range and resistant to alternating cold and hot conditions, the raw material formula composition of which is shown in Table 4 below, the soft monomer is butyl acrylate; the hard monomer is methyl methacrylate; the functional monomer is acrylic acid; the solvent is dimethyl carbonate and ethyl acetate, and the weight ratio is 5:3. The raw materials are calculated by weight, as follows:

[0071] Table 4

[0072]

[0073]

[0074] A method for preparing a TPU pressure-sensitive adhesive for car covers that is resistant to alternating hot and cold temperatures over a wide temperature range, comprising the following steps:

[0075] (1) After uniformly mixing the soft monomer, hard monomer, functional monomer, solvent, initiator, and acrylic rubber according to a certain proportion, a reactant A is obtained, and the reactant A is evenly divided into two parts;

[0076] (2) adding a portion of the mixture into a reaction flask and heating the mixture to reflux the mixture. The reaction was maintained at 84° C. for 60 minutes to obtain reactant B.

[0077] (3) Then, another portion of reactant A is added dropwise to reactant B obtained in step 2 for 120 minutes. After the addition is completed, the temperature is kept at 84° C. for 4 hours, then cooled to 25° C., and stirred evenly after cooling to obtain the product.

[0078] A method for using a TPU car cover pressure-sensitive adhesive that is resistant to alternating hot and cold temperatures over a wide temperature range comprises adding a curing agent and a solvent into the pressure-sensitive adhesive and stirring the mixture evenly, and coating the mixture on a TPU film using a coating machine.

[0079] The curing agent is an ethyl acetate solution of aluminum acetylacetonate with a mass concentration of 5%;

[0080] The solvent is ethyl acetate;

[0081] The amount of the curing agent used is 2wt% of the weight of the pressure-sensitive adhesive, and the weight ratio of the solvent to the adhesive is 1:1.

[0082] The pressure-sensitive adhesive prepared in Examples 7-12 and Comparative Examples 4-5 was used for high and low temperature cycle test. ① The sample was pasted on the steel plate according to the peel strength test sample, and the adhesiveness was observed after normal tearing; ② The sample was prepared into a TPU bonding test sample, and the TPU bonding performance was tested after the test; ③ The adhesive was prepared into a TPU car cover sample, and the initial adhesion, peel strength and lasting adhesion were tested after the test. The test was carried out in a wet heat cycle test box (-40℃ (humidity 0) cooling for 1h and maintaining for 4h, 65℃ (humidity 50% RH) heating for 1h and maintaining for 4h) for 100 cycles. After the placement, the corresponding performance tests of the three groups of samples were tested and the test results were recorded in the following Table 5.

[0083] Table 5

[0084]

[0085]

Claims

1. A TPU pressure-sensitive adhesive for car covers with wide temperature range and resistant to alternating hot and cold, characterized in that: The raw materials for preparation include, by weight: 13-24 parts of soft monomer, 7-8.5 parts of hard monomer, 0.1-3 parts of functional monomer, 70 parts of solvent, 0.01-0.05 parts of initiator, and 0.5-3 parts of acrylic rubber; The soft monomer is butyl acrylate; the hard monomer is methyl methacrylate; the functional monomer is acrylic acid; the solvent is a combination of dimethyl carbonate and ethyl acetate, with a weight ratio of (1-10):3; The acrylic rubber is selected from one or a combination of AR74 of Japan Zeon Co., Ltd., AR840 of Japan Toa Paint Co., Ltd., AR100 of Sichuan Suining Qinglong Acrylic Rubber Factory, and AR96 of Chongqing Jianfeng Co., Ltd.

2. According to claim 1, the TPU pressure-sensitive adhesive for car cover with wide temperature range and resistance to alternating hot and cold, characterized in that: The initiator is selected from one or a combination of organic peroxide initiators, inorganic peroxide initiators and azo initiators.

3. The TPU pressure-sensitive adhesive for car cover with wide temperature range and resistance to alternating hot and cold conditions according to claim 1, characterized in that: The organic peroxide initiator is selected from one or a combination of benzoyl peroxide, dilauroyl peroxide, cumene hydroperoxide, tert-butyl perbenzoate, and tert-amyl peroxide 2-ethylhexanoate.

4. A method for preparing the TPU pressure-sensitive adhesive for car cover with wide temperature range and resistant to alternating hot and cold according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) After uniformly mixing the soft monomer, hard monomer, functional monomer, solvent, initiator and acrylic rubber according to the proportion, a reactant A is obtained, which is then divided into two parts; (2) adding a portion of the mixture into a reaction flask and heating the mixture to reflux the mixture. The reaction is maintained at 80-90°C for 30-90 minutes to obtain reactant B. (3) Then, another portion of reactant A is added dropwise to reactant B obtained in step 2 for 60-180 minutes. After the addition is completed, the temperature is kept at 80-90°C for 3-5 hours, then cooled to room temperature, and stirred evenly after cooling to obtain the product.

5. A method for using the TPU pressure-sensitive adhesive for car covers with wide temperature range and resistance to alternating hot and cold conditions according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: adding a curing agent and an organic solvent into the pressure-sensitive adhesive and stirring the mixture evenly, coating the mixture on a TPU film with a coating machine, and curing the mixture to obtain the product.

6. The method for using the TPU pressure-sensitive adhesive for car covers with wide temperature range and resistance to alternating hot and cold conditions according to claim 5, characterized in that: The mass of the curing agent is 0.5-5wt% of the weight of the pressure-sensitive adhesive.

Citation Information

Patent Citations

  • Method for preparing high-strength heat-resistant silicon resin modified acrylic ester pressure-sensitive adhesive

    CN101979454A

  • Alternating cold and heat resistant removable acrylic pressure sensitive adhesive and preparation method and application thereof

    CN109825224A

  • Solvent type acrylate pressure-sensitive adhesive based on TPU base material and preparation method thereof

    CN107629738A

  • Solvent-type acrylate pressure-sensitive adhesive suitable for adhering TPU, and preparation method thereof

    CN108048006A

  • Acrylate pressure-sensitive adhesive with thin adhesive layer and high peel strength and preparation method of acrylate pressure-sensitive adhesive

    CN110964465A