Substrate processing method, semiconductor device manufacturing method, recording medium, and substrate processing apparatus

By controlling the temperature and gas supply time in stages, the problems of diffusion of Mo-containing films at high temperatures and slow reaction at low temperatures were solved, achieving the effects of inhibiting diffusion and improving productivity.

CN115989338BActive Publication Date: 2026-11-17KOKUSAI DENKI KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202080103424.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-23
Publication Date
2026-11-17
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

When forming a Mo-containing film using Mo-containing gas and reducing gas on a base film, if the film is formed at high temperature, the element diffusion in the base film is severe; if the film is formed at low temperature, the reaction rate is slow, resulting in a decrease in productivity.

Method used

A method of controlling substrate temperature and gas supply time in stages is adopted. First, a first Mo-containing film is formed at a low temperature. Then, the temperature is adjusted and a second Mo-containing film is formed at a high temperature. The final film is formed by multiple cycles of gas supply.

Benefits of technology

It effectively inhibits the diffusion of metal elements from the substrate metal film, improves productivity, and ensures film quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115989338B_ABST
    Figure CN115989338B_ABST
Patent Text Reader

Abstract

This invention can suppress the diffusion of metal elements from a molybdenum-containing substrate metal film and improve productivity. It includes the following steps: (a) placing a substrate in a processing chamber; (b1) adjusting the substrate to a first temperature; (b2) supplying a molybdenum-containing gas to the substrate; (b3) supplying a reducing gas to the substrate for a first time; (b4) after (b1), forming a first molybdenum-containing film on the substrate by performing (b2) and (b3) at least once; (c1) after (b4), adjusting the substrate to a second temperature; (c2) supplying a molybdenum-containing gas to the substrate; (c3) supplying a reducing gas to the substrate for a second time; and (c4) after (c1), forming a second molybdenum-containing film on the first molybdenum-containing film by performing (c2) and (c3) at least once.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a substrate processing method, a method for manufacturing a semiconductor device, a recording medium, and a substrate processing apparatus. Background Technology

[0002] As word lines for NAND flash memory or DRAM with a 3D structure, a low-resistance tungsten (W) film is used, for example. In addition, sometimes a barrier film, such as a titanium nitride (TiN) film or a molybdenum (Mo) film, is formed between the W film and the insulating film (see, for example, Patent Document 1 and Patent Document 2).

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2011-66263

[0006] Patent Document 2: International Publication No. 2019 / 058608 Summary of the Invention

[0007] The problem that the invention aims to solve

[0008] However, when forming a Mo-containing film using Mo-containing gas and reducing gas on a basement membrane, if film formation is carried out at high temperatures, elements contained in the basement membrane diffuse from the basement membrane to the Mo-containing film. On the other hand, if film formation is carried out at low temperatures, the diffusion of elements contained in the basement membrane from the basement membrane decreases, but the reaction between the Mo-containing gas and the reducing gas is slow, requiring a longer supply time.

[0009] The purpose of this disclosure is to provide a technology that can suppress the diffusion of metal elements from a molybdenum-containing substrate metal film and improve productivity.

[0010] Methods for solving problems

[0011] According to one aspect of this disclosure, a technique is provided comprising the following steps: (a) placing a substrate in a processing chamber; (b1) adjusting the substrate to a first temperature; (b2) supplying the substrate with a molybdenum-containing gas; (b3) supplying the substrate with a reducing gas for a first time; (b4) after (b1), forming a first molybdenum-containing film on the substrate by performing (b2) and (b3) more than once; (c1) after (b4), adjusting the substrate to a second temperature; (c2) supplying the substrate with the molybdenum-containing gas; (c3) supplying the substrate with the reducing gas for a second time; and (c4) after (c1), forming a second molybdenum-containing film on the first molybdenum-containing film by performing (c2) and (c3) more than once.

[0012] Invention Effects

[0013] According to this disclosure, diffusion from a molybdenum-containing substrate metal film can be suppressed, and productivity can be improved. Attached Figure Description

[0014] Figure 1 This is a schematic longitudinal sectional view of a vertical processing furnace of a substrate processing apparatus according to one embodiment of the present disclosure.

[0015] Figure 2 yes Figure 1 A rough cross-sectional view along line AA in the diagram.

[0016] Figure 3 This is a schematic structural diagram of the controller of the substrate processing apparatus in one embodiment of the present disclosure, and is a diagram of the control system of the controller shown in block diagram.

[0017] Figure 4 This is a diagram illustrating a substrate processing step in one embodiment of the present disclosure.

[0018] Figure 5 (A) is a cross-sectional view of the substrate before the formation of the first Mo-containing film on the substrate. Figure 5 (B) is a cross-sectional view of the substrate in the case where a first Mo-containing film is formed on the substrate. Figure 5 (C) is a cross-sectional view of the substrate in the case where a second Mo-containing film is formed on the first Mo-containing film.

[0019] Figure 6 This is a diagram illustrating a modified example of the second Mo-containing film formation step in the substrate processing steps of one embodiment of the present disclosure. Detailed Implementation

[0020] The following is for reference Figures 1-5 This explanation is provided. Furthermore, the accompanying drawings used in the following explanation are schematic, and the dimensional relationships and ratios of the elements shown in the drawings may not correspond to reality. Additionally, the dimensional relationships and ratios of elements may not be consistent across different drawings.

[0021] (1) Structure of the substrate processing device

[0022] The substrate processing apparatus 10 includes a processing furnace 202 equipped with a heater 207, which serves as a heating unit (heating mechanism, heating system). The heater 207 is cylindrical and is vertically mounted by means of a heater base (not shown) that serves as a holding plate.

[0023] An outer tube 203, concentrically arranged with the heater 207, forms a reaction vessel (processing vessel) inside the heater 207. The outer tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC), and is formed into a cylindrical shape that is closed at the top and open at the bottom. Below the outer tube 203, a manifold (inlet flange) 209 is arranged concentrically with the outer tube 203. The manifold 209 is made of a metal such as stainless steel (SUS), and is formed into a cylindrical shape that is open at both the top and bottom. An O-ring 220a, serving as a sealing component, is provided between the upper end of the manifold 209 and the outer tube 203. By supporting the manifold 209 on the heater base, the outer tube 203 is installed vertically.

[0024] An inner tube 204, constituting a reaction vessel, is disposed inside the outer tube 203. The inner tube 204 is made of heat-resistant materials such as quartz (SiO2) or silicon carbide (SiC), and is formed into a cylindrical shape that is closed at the top and open at the bottom. The processing vessel (reaction vessel) is mainly composed of the outer tube 203, the inner tube 204, and the manifold 209. A processing chamber 201 is formed in the hollow part of the processing vessel (inside the inner tube 204).

[0025] The processing chamber 201 is configured to accommodate a wafer 200, which serves as a substrate, arranged in a horizontal orientation in a multi-layered manner in the vertical direction via a crystal boat 217, which will be described later.

[0026] Inside the processing chamber 201, nozzles 410 and 420 are provided so as to penetrate the side wall of the manifold 209 and the inner pipe 204. The nozzles 410 and 420 are connected to the gas supply pipes 310 and 320, respectively. However, the processing furnace 202 of this embodiment is not limited to the above-described manner.

[0027] Mass flow controllers (MFCs) 312 and 322, serving as flow controllers (flow control units), are sequentially installed on gas supply pipes 310 and 320, starting from the upstream side. Additionally, valves 314 and 324, serving as on / off valves, are installed on gas supply pipes 310 and 320, respectively. Gas supply pipes 510 and 520, supplying inert gas, are connected downstream of valves 314 and 324 on gas supply pipes 310 and 320, respectively. On gas supply pipes 510 and 520, MFCs 512 and 522, serving as flow controllers (flow control units), and valves 514 and 524, serving as on / off valves, are sequentially installed on the upstream side.

[0028] Nozzles 410 and 420 are connected to the front ends of gas supply pipes 310 and 320, respectively. Nozzles 410 and 420 are configured as L-shaped nozzles, with their horizontal portions extending through the side wall of manifold 209 and inner pipe 204. The vertical portions of nozzles 410 and 420 are disposed inside a preparation chamber 201a, which is a channel-shaped (groove-shaped) chamber that protrudes radially outward from the inner pipe 204 and extends vertically. Inside the preparation chamber 201a, nozzles are disposed upward along the inner wall of the inner pipe 204 (above the arrangement direction of the wafers 200).

[0029] Nozzles 410 and 420 are arranged to extend from the lower region to the upper region of the processing chamber 201, and multiple gas supply holes 410a and 420a are respectively provided at positions opposite to the wafer 200. Processing gas is supplied to the wafer 200 through the gas supply holes 410a and 420a of the nozzles 410 and 420. Multiple gas supply holes 410a and 420a are provided from the lower to the upper part of the inner tube 204, each having the same opening area and the same opening spacing. However, the gas supply holes 410a and 420a are not limited to the above arrangement. For example, the opening area can gradually increase from the lower part to the upper part of the inner tube 204. This allows for a more uniform flow rate of gas supplied from the gas supply holes 410a and 420a.

[0030] The gas supply holes 410a and 420a of the nozzles 410 and 420 are provided at a height from the lower part to the upper part of the wafer 217 (described later). Therefore, the processing gas supplied from the gas supply holes 410a and 420a of the nozzles 410 and 420 into the processing chamber 201 is supplied to the entire area of ​​the wafer 200 housed in the wafer 217 from the lower part to the upper part. The nozzles 410 and 420 can be provided in such a way that they extend from the lower region to the upper region of the processing chamber 201, but it is preferable that they extend to near the top of the wafer 217.

[0031] Raw material gas is supplied as processing gas from gas supply pipe 310 through MFC 312, valve 314, and nozzle 410 into processing chamber 201.

[0032] Reducing gas is supplied as processing gas from gas supply pipe 320 through MFC 322, valve 324, and nozzle 420 into processing chamber 201.

[0033] Rare gases, such as argon (Ar), are supplied as inert gases into the processing chamber 201 through gas supply pipes 510 and 520 via MFCs 512 and 522, valves 514 and 524, and nozzles 410 and 420, respectively. The following description uses Ar gas as an example of an inert gas; however, in addition to Ar gas, rare gases such as helium (He), neon (Ne), and xenon (Xe) can also be used as inert gases.

[0034] The processing gas supply system mainly consists of gas supply pipes 310 and 320, MFCs 312 and 322, valves 314 and 324, and nozzles 410 and 420. However, nozzles 410 and 420 can also be considered as the processing gas supply system alone. The processing gas supply system can also be simply referred to as the gas supply system. When Mo-containing gas flows through gas supply pipe 310, the Mo-containing gas supply system mainly consists of gas supply pipe 310, MFC 312, and valve 314. However, nozzle 410 can also be included in the Mo-containing gas supply system. Similarly, when reducing gas flows through gas supply pipe 320, the reducing gas supply system mainly consists of gas supply pipe 320, MFC 322, and valve 324. However, nozzle 420 can also be included in the reducing gas supply system. Furthermore, the inert gas supply system mainly consists of gas supply pipes 510 and 520, MFCs 512 and 522, and valves 514 and 524. The inert gas supply system can also be called the rare gas supply system.

[0035] In this embodiment, the gas supply method involves conveying gas via nozzles 410 and 420 within a preparatory chamber 201a located within an annular, elongated space defined by the inner wall of the inner tube 204 and the ends of multiple wafers 200. Then, gas is ejected into the inner tube 204 from multiple gas supply holes 410a and 420a located opposite the wafers on the nozzles 410 and 420. More specifically, processing gas is ejected through the gas supply holes 410a of the nozzles 410 and 420a of the nozzles 420 in a direction parallel to the surface of the wafers 200.

[0036] The exhaust port (exhaust outlet) 204a is a through-hole formed on the side wall of the inner tube 204, opposite to the nozzles 410 and 420. For example, it is a narrow, slit-like through-hole that is elongated in the vertical direction. Gas supplied from the gas supply holes 410a and 420a of the nozzles 410 and 420 into the processing chamber 201 and flowing on the surface of the wafer 200 flows through the exhaust port 204a into the exhaust path 206 formed by the gap between the inner tube 204 and the outer tube 203. Then, the gas flowing into the exhaust path 206 flows into the exhaust pipe 231 and is discharged out of the processing furnace 202.

[0037] The vent 204a is positioned opposite to the plurality of wafers 200. Gas supplied from the gas supply holes 410a and 420a to the vicinity of the wafers 200 in the processing chamber 201 flows horizontally and then flows through the vent 204a into the exhaust path 206. The vent 204a is not limited to being configured as a slit-shaped through hole, but may also be composed of multiple holes.

[0038] An exhaust pipe 231 for venting the atmosphere inside the processing chamber 201 is provided in the manifold 209. From upstream, the exhaust pipe 231 is sequentially connected to a pressure sensor 245 (a pressure detector, or pressure sensing unit) for detecting the pressure inside the processing chamber 201, an APC (Auto Pressure Controller) valve 243, and a vacuum pump 246 (a vacuum venting device). The APC valve 243 can perform vacuum venting and stop vacuum venting in the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is operating. Furthermore, the pressure inside the processing chamber 201 can be adjusted by regulating the valve opening while the vacuum pump 246 is operating. The exhaust system mainly consists of an exhaust port 204a, an exhaust path 206, an exhaust pipe 231, an APC valve 243, and a pressure sensor 245. It is also possible to include the vacuum pump 246 in the exhaust system.

[0039] A sealing cover 219, serving as a furnace opening cover, is provided below the manifold 209 to airtightly seal the lower opening of the manifold 209. The sealing cover 219 is configured to abut against the lower end of the manifold 209 from the lower vertical direction. The sealing cover 219 is made of a metal such as SUS and is formed in a disc shape. An O-ring 220b, serving as a sealing member, is provided on the upper surface of the sealing cover 219 and abuts against the lower end of the manifold 209. On the side of the sealing cover 219 opposite to the processing chamber 201, a rotation mechanism 267 is provided to rotate a wafer boat 217 containing the wafer 200. The rotation shaft 255 of the rotation mechanism 267 passes through the sealing cover 219 and is connected to the wafer boat 217. The rotation mechanism 267 is configured to rotate the wafer 200 by rotating the wafer boat 217. The sealing cover 219 is configured to be raised and lowered in the vertical direction via a crystal boat lift 115, which is vertically mounted outside the outer tube 203 and serves as a lifting mechanism. The crystal boat lift 115 is configured to move the crystal boat 217 in and out of the processing chamber 201 by raising and lowering the sealing cover 219. The crystal boat lift 115 is configured as a conveying device (conveyor system) for conveying the crystal boat 217 and the wafer 200 housed within the crystal boat 217 in and out of the processing chamber 201.

[0040] The crystal boat 217, serving as a substrate support, is configured such that multiple wafers 200, for example 25 to 200, are arranged horizontally and aligned with each other at intervals in the vertical direction. The crystal boat 217 is made of heat-resistant materials such as quartz or SiC. At the lower part of the crystal boat 217, a heat insulation plate 218, made of heat-resistant materials such as quartz or SiC, is supported horizontally in multiple layers (not shown). According to this structure, heat from the heater 207 is difficult to transfer to the sealing cover 219 side. However, this embodiment is not limited to the above-described manner. For example, instead of providing the heat insulation plate 218 at the lower part of the crystal boat 217, a heat insulation cylinder may be provided, which is configured as a cylindrical component made of heat-resistant materials such as quartz or SiC.

[0041] like Figure 2 As shown, a temperature sensor 263, which serves as a temperature detector, is installed inside the inner tube 204. The electrical current supplied to the heater 207 is adjusted based on the temperature information detected by the temperature sensor 263, thereby achieving the desired temperature distribution within the processing chamber 201. The temperature sensor 263, like the nozzles 410 and 420, is configured in an L-shape and is installed along the inner wall of the inner tube 204.

[0042] like Figure 3 As shown, the controller 121, serving as the control unit (control unit), is configured as a computer equipped with a CPU (Central Processing Unit) 121a, RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, storage device 121c, and I / O port 121d are configured to exchange data with the CPU 121a via an internal bus. The controller 121 is connected, for example, to an input / output device 122 configured as a touch panel or the like.

[0043] The storage device 121c is configured such as flash memory or HDD (Hard Disk Drive). The storage device 121c stores, in a readable manner, a control program that controls the operation of the substrate processing device, and a process flow that describes the steps and conditions of the semiconductor device manufacturing method (described later). The process flow is a combination of methods that enable the controller 121 to execute each step in the semiconductor device manufacturing method (described later) to obtain a predetermined result, and functions as a program. Hereinafter, the process flow, control program, etc., will be collectively referred to as a program. When the term "program" is used in this specification, sometimes only the process flow is included, sometimes only the control program is included, or sometimes a combination of the process flow and the control program is included. RAM 121b is configured as a storage area (working area) for temporarily holding programs, data, etc., read by the CPU 121a.

[0044] I / O port 121d is connected to the aforementioned MFC312, 322, 512, 522, valves 314, 324, 514, 524, pressure sensor 245, APC valve 243, vacuum pump 246, heater 207, temperature sensor 263, rotating mechanism 267, crystal boat lift 115, etc.

[0045] CPU 121a is configured to read and execute control programs from storage device 121c, and to read process data from storage device 121c based on input instructions from input / output device 122. According to the read process data, CPU 121a controls various gas flow adjustment operations using MFCs 312, 322, 512, and 522; opening and closing operations of valves 314, 324, 514, and 524; opening and closing operations of APC valve 243; pressure adjustment operations based on pressure sensor 245 using APC valve 243; temperature adjustment operations of heater 207 based on temperature sensor 263; starting and stopping of vacuum pump 246; rotation and speed adjustment operations of crystal boat 217 using rotating mechanism 267; lifting and lowering operations of crystal boat 217 using crystal boat elevator 115; and the receiving operations of wafer 200 into crystal boat 217.

[0046] The controller 121 is configured to install the aforementioned program stored in an external storage device (e.g., magnetic tape, floppy disk, hard disk, CD, DVD, MO, USB memory, memory card, etc.) 123 onto a computer. The storage device 121c and the external storage device 123 constitute a computer-readable recording medium. Hereinafter, they will be collectively referred to as the recording medium. In this specification, the recording medium may sometimes contain only the storage device 121c, sometimes only the external storage device 123, or sometimes both. Providing the program to the computer may also be done without using the external storage device 123, but rather using communication means such as the Internet or a dedicated line.

[0047] (2) Substrate processing process

[0048] As a step in the manufacturing process of semiconductor devices, using Figure 4 , Figure 5 (A) Figure 5 (C) An example of a process for forming a molybdenum (Mo)-containing film on wafer 200, for example, as a control gate electrode for a 3D NAND, will be described. Here, as Figure 5As shown in (A), a wafer 200 with an aluminum oxide (AlO) film containing aluminum (Al), a non-transition metal element, formed on its surface is used. The process of forming the Mo-containing film is performed using the processing furnace 202 of the substrate processing apparatus 10 described above. In the following description, the operation of each part constituting the substrate processing apparatus 10 is controlled by the controller 121.

[0049] The substrate processing step (semiconductor device manufacturing step) of this embodiment includes the following steps:

[0050] (a) A process of housing a wafer 200 in a processing chamber 201, which serves as a processing container;

[0051] (b1) The process of adjusting wafer 200 to the first temperature;

[0052] (b2) The process of supplying Mo-containing gas to wafer 200;

[0053] (b3) The process of supplying reducing gas to wafer 200 immediately;

[0054] (b4) After (b1), a process of forming a first Mo-containing film on wafer 200 is performed by performing (b2) and (b3) more than once;

[0055] (c1) The process of adjusting wafer 200 to the second temperature after (b4);

[0056] (c2) The process of supplying Mo-containing gas to wafer 200;

[0057] (c3) The process of supplying a second reducing gas to wafer 200; and

[0058] (c4) After (c1), a process of forming a second Mo-containing film on the first Mo-containing film by performing (c2) and (c3) more than once.

[0059] In addition, the second temperature is higher than the first temperature, and the second time is shorter than the first time.

[0060] In this specification, the term "wafer" sometimes refers to "the wafer itself" and sometimes to "a laminate of a wafer and a specified layer, film, etc., formed on its surface." Similarly, the term "surface of a wafer" sometimes refers to "the surface of the wafer itself" and sometimes to "the surface of a specified layer, film, etc., formed on the wafer." The use of the term "substrate" in this specification is synonymous with the use of the term "wafer."

[0061] (Wafer loading)

[0062] When multiple wafers 200 are loaded (wafer loading) into the crystal boat 217, such as Figure 1 As shown, the crystal boat 217 supporting multiple wafers 200 is lifted by the crystal boat elevator 115, moved (crystal boat loading) into the processing chamber 201, and stored in the processing container. In this state, the sealing cap 219 closes the lower opening of the outer tube 203 via the O-ring 220.

[0063] (Pressure and temperature adjustment)

[0064] Vacuum pump 246 is used to exhaust vacuum, so that the space inside processing chamber 201, i.e., the space where wafer 200 exists, reaches the desired pressure (vacuum level). At this time, the pressure inside processing chamber 201 is measured by pressure sensor 245, and based on the measured pressure information, APC valve 243 is controlled by feedback (pressure adjustment). Vacuum pump 246 remains operational at least until the processing of wafer 200 is completed.

[0065] Additionally, heating is performed by heater 207 to bring the processing chamber 201 to a desired temperature. At this time, feedback control (temperature adjustment) is applied to the power supply to heater 207 based on temperature information detected by temperature sensor 263 to achieve the desired temperature distribution within the processing chamber 201. Heating within the processing chamber 201 by heater 207 continues at least until the processing of wafer 200 is completed; however, until the first Mo-containing film formation process described later is completed, the temperature of heater 207 is adjusted to ensure that the temperature of wafer 200 is within a first temperature range of 445°C or higher and 505°C or lower.

[0066] [First Mo-containing film formation process]

[0067] (Including Mo gas supply, step S11)

[0068] Valve 314 is opened, allowing the Mo-containing gas, used as the raw material gas, to flow within the gas supply pipe 310. The Mo-containing gas, with its flow rate regulated by MFC 312, is supplied to the processing chamber 201 from the gas supply port 410a of nozzle 410 and discharged from exhaust pipe 231. At this time, Mo-containing gas is supplied to wafer 200. Simultaneously, valve 514 is opened, allowing an inert gas such as Ar to flow within the gas supply pipe 510. The Ar gas flowing within the gas supply pipe 510, with its flow rate regulated by MFC 512, is supplied to the processing chamber 201 along with the Mo-containing gas and discharged from exhaust pipe 231. To prevent Mo-containing gas from entering nozzle 420, valve 524 is opened, allowing Ar gas to flow within the gas supply pipe 520. The Ar gas is supplied to the processing chamber 201 via gas supply pipe 320 and nozzle 420 and discharged from exhaust pipe 231.

[0069] At this time, the APC valve 243 is adjusted so that the pressure in the processing chamber 201 is, for example, within the range of 1 to 3990 Pa, and for example, 1000 Pa. The supply flow rate of the Mo-containing gas controlled by the MFC 312 is, for example, within the range of 0.1 to 1.0 slm, preferably 0.1 to 0.5 slm. The supply flow rates of the Ar gas controlled by the MFCs 512 and 522 are respectively set to, for example, within the range of 0.1 to 20 slm. Furthermore, the expression of a numerical range such as "1 to 3990 Pa" in this disclosure means that the lower limit and the upper limit are included in this range. Therefore, for example, "1 to 3990 Pa" means "more than 1 Pa and less than 3990 Pa". The same applies to other numerical ranges.

[0070] At this time, the gases flowing within the processing chamber 201 are only Mo-containing gas and Ar gas. Here, the Mo-containing gas used as the feed gas can be a molybdenum (Mo)-containing gas containing molybdenum (Mo) and oxygen (O). Examples of Mo-containing gases include molybdenum dioxide dichlorodioxide (MoO2Cl2) gas and molybdenum tetrachlorodioxide (MoOCl4) gas. Here, the case where MoO2Cl2 gas is used as the Mo-containing gas will be explained. By supplying MoO2Cl2 gas, a Mo-containing layer is formed on the wafer 200 (which serves as the substrate film on the surface of the AlO film). The Mo-containing layer can be a Mo layer containing Cl and O, an adsorption layer of MoO2Cl2, or both.

[0071] (Residual gas removed, step S12)

[0072] After a predetermined time elapsed since the start of Mo-containing gas supply, for example, 1 to 60 seconds, valve 314 of gas supply pipe 310 is closed to stop the supply of Mo-containing gas. That is, the time for supplying Mo-containing gas to wafer 200 is, for example, 1 to 60 seconds. At this time, APC valve 243 of exhaust pipe 231 is kept open, and vacuum pump 246 is used to evacuate the processing chamber 201, removing any unreacted or Mo-containing gases remaining in the processing chamber 201 that may contribute to the formation of the Mo-containing layer. In other words, the processing chamber 201 is purged. At this time, valves 514 and 524 remain open, maintaining the supply of Ar gas to the processing chamber 201. Ar gas acts as a purging gas, which can improve the effect of removing any unreacted or Mo-containing gases remaining in the processing chamber 201 that may contribute to the formation of the Mo-containing layer.

[0073] (Supply reducing gas, step S13)

[0074] After removing residual gas from processing chamber 201, valve 324 is opened to allow reducing gas to flow in gas supply pipe 320. The reducing gas flow rate is regulated by MFC 322 and supplied to processing chamber 201 from gas supply port 420a of nozzle 420, and discharged from exhaust pipe 231. At this time, reducing gas is supplied to wafer 200. Simultaneously, valve 524 is opened to allow Ar gas to flow in gas supply pipe 520. The Ar gas flowing in gas supply pipe 520 is flow rate regulated by MFC 522. Ar gas and reducing gas are supplied to processing chamber 201 together and discharged from exhaust pipe 231. At this time, to prevent reducing gas from entering nozzle 410, valve 514 is opened to allow Ar gas to flow in gas supply pipe 510. Ar gas is supplied to processing chamber 201 via gas supply pipe 310 and nozzle 410 and discharged from exhaust pipe 231.

[0075] At this time, the APC valve 243 is adjusted to bring the pressure inside the processing chamber 201 to a range of, for example, 1 to 3990 Pa, and preferably 2000 Pa. The supply flow rate of the reducing gas controlled by the MFC 322 is, for example, 1 to 50 slm, preferably 15 to 30 slm. The supply flow rate of Ar gas controlled by the MFCs 512 and 522 is set to a range of, for example, 0.1 to 30 slm. At this time, the time for supplying the reducing gas to the wafer 200 is a time of 5 minutes to 30 minutes as the first time, for example, 20 minutes. By setting the time for supplying the reducing gas to the wafer 200 to 5 minutes or more, the Mo-containing gas adsorbed on the wafer 200 can be reduced; by setting it to 30 minutes or less, throughput can be increased and productivity ensured.

[0076] At this time, the gases flowing inside the processing chamber 201 are only reducing gas and Ar gas. For example, hydrogen (H2) gas (containing hydrogen (H) gas), deuterium (D2) gas, or gas containing activated hydrogen can be used as the reducing gas. Here, the case of using H2 gas as the reducing gas will be described as an example. The H2 gas undergoes a displacement reaction with at least a portion of the Mo-containing layer formed on the wafer 200 in step S11. That is, O and chlorine (Cl) in the Mo-containing layer react with H2, detach from the Mo layer, and are discharged from the processing chamber 201 as reaction byproducts such as water vapor (H2O), hydrogen chloride (HCl), and chlorine (Cl2). Then, a Mo-containing layer that is substantially free of Cl and O is formed on the wafer 200.

[0077] (Residual gas removal, step S14)

[0078] After the Mo-containing layer is formed, valve 324 is closed to stop the supply of reducing gas.

[0079] Then, through the same processing steps as step S12 described above, unreacted gases or reducing gases and reaction byproducts remaining in the processing chamber 201 that contribute to the formation of the Mo-containing layer are removed from the processing chamber 201. That is, the processing chamber 201 is purged.

[0080] (Number of times specified)

[0081] By performing the above steps S11 to S14 in a loop at least once (a specified number of times (n times)), as follows: Figure 5 As shown in (B), a first Mo-containing film of a specified thickness (e.g., 1–5 nm) is formed on a wafer 200 on which an AlO film is formed. The above cycle is preferably repeated multiple times.

[0082] Here, compared to a Mo-containing film formed by heating the wafer 200 at a temperature below 445°C or above 505°C, the surface roughness of the Mo-containing film surface is deteriorated when the temperature of the wafer 200 is heated to a temperature within the range of 445°C to 505°C. Furthermore, compared to a Mo-containing film formed by heating the wafer 200 at a temperature below 445°C or above 505°C, the diffusion of Al from the substrate AlO film into the film is increased when the temperature of the wafer 200 is heated to a temperature within the range of 445°C to 505°C. This is believed to be because, at temperatures below 445°C, the reduction based on the H2 gas supply in step S13 is incomplete, and the Mo-containing gas is not sufficiently reduced, resulting in the formation of MoO. x Cl y The AlO film on the substrate, and the Mo-containing film formed therefrom, are covered by MoO. x Cl y Erosion. In this disclosure, "erosion" refers to reduction. Furthermore, it is believed that the reason is that at temperatures above 505°C, the AlO film on the substrate or the Mo-containing film formed therefrom will be eroded by HCl generated as a reaction byproduct due to the supply of reducing gas in step S13.

[0083] That is, in the first Mo-containing film formation process described above, by setting the wafer 200 to a temperature within the range of 445°C or higher and 505°C or lower, a first Mo-containing film is formed on the wafer 200 on which an AlO film is formed, thereby suppressing the diffusion of Al from the substrate AlO film into the Mo-containing film. In other words, the first Mo-containing film is a film capable of suppressing the diffusion of Al from the substrate AlO film, and thus becomes a low-resistance film. Furthermore, the first Mo-containing film is a flat film with good surface roughness, having an average surface roughness Ra of 1.0 nm or lower.

[0084] (Pressure and temperature adjustment)

[0085] After forming a first Mo-containing film of a specified thickness on wafer 200, rare gas Ar, acting as an inert gas, is supplied into processing chamber 201 through gas supply pipes 510 and 520, and discharged through exhaust pipe 231. Ar gas acts as a purging gas, thereby purging processing chamber 201 with inert gas, removing residual gases and reaction byproducts from processing chamber 201. Subsequently, the atmosphere in processing chamber 201 is replaced with inert gas (inert gas replacement). Under this inert gas atmosphere, the pressure in processing chamber 201 is measured by pressure sensor 245. Based on this measured pressure information, feedback control (pressure adjustment) is applied to APC valve 243. At this time, APC valve 243 is adjusted so that the pressure in processing chamber 201 is at least higher than the pressure in the first Mo-containing film formation process and the pressure in the second Mo-containing film formation process (described later), for example, atmospheric pressure. By raising the pressure in processing chamber 201 to a level higher than the pressure in the film formation process, thermal conductivity can be improved and the heating time shortened. Furthermore, to improve thermal conductivity, the pressure here can be increased to near atmospheric pressure. Additionally, in this process, by using a rare gas, changes in the surface properties of the first Mo-containing film can be suppressed. For example, when nitrogen (N2), which is commonly used as an inert gas, is used, the first Mo-containing film reacts with N2 (adsorption), affecting its surface properties. On the other hand, using a rare gas such as Ar can suppress such changes in surface properties.

[0086] Additionally, at this time, heating is performed by heater 207 to bring the processing chamber 201 to the desired temperature. Feedback control (temperature adjustment) is applied to the power supply to heater 207 based on temperature information detected by temperature sensor 263 to achieve the desired temperature distribution within the processing chamber 201. Hereinafter, the temperature of heater 207 is set to a second temperature, i.e., a temperature between 550°C and 590°C, higher than the first temperature, such as 580°C. That is, during the period before the completion of the second Mo-containing film formation process (described later), the temperature of heater 207 is adjusted to a temperature within the second range of 550°C and 590°C, such as 580°C, where the temperature of wafer 200 is at least 550°C and less than 590°C.

[0087] Furthermore, at this time, when using N2 gas as an inert gas, the first Mo-containing film formed on the wafer 200 is nitrided. In this disclosure, by using Ar gas as an inert gas, the wafer 200 can be heated without changing the surface state of the first Mo-containing film. Alternatively, a reducing gas can be used for heating. That is, the wafer 200 is heated from a first temperature to a second temperature in a reducing atmosphere. By heating in such a reducing atmosphere, byproducts and impurities contained in the first Mo-containing film can be removed while heating. That is, annealing can be performed during heating. By performing annealing, at least the byproducts and impurities adsorbed on the surface of the first Mo-containing film can be removed.

[0088] [Second Mo-containing film formation process]

[0089] (Supply gas containing Mo membrane, step S21)

[0090] Valve 314 is opened to allow the Mo-containing gas, which serves as the raw material gas, to flow within the gas supply pipe 310. Furthermore, the Mo-containing gas used in the second Mo-containing film formation process can be the same gas used in the first Mo-containing film formation process, or it can be a different type of Mo-containing gas. The Mo-containing gas is regulated by MFC 312 and supplied to the processing chamber 201 from the gas supply port 410a of nozzle 410, and discharged from exhaust pipe 231. At this time, Mo-containing gas is supplied to wafer 200. Simultaneously, valve 514 is opened to allow an inert gas such as Ar to flow within the gas supply pipe 510. The Ar gas flowing within the gas supply pipe 510 is regulated by MFC 512 and supplied to the processing chamber 201 along with the Mo-containing gas, and discharged from exhaust pipe 231. At this time, to prevent Mo-containing gas from entering nozzle 420, valve 524 is opened to allow Ar gas to flow within the gas supply pipe 520. Ar gas is supplied into the processing chamber 201 through the gas supply pipe 320 and the nozzle 420, and is discharged from the exhaust pipe 231.

[0091] At this time, adjust APC valve 243 to make the pressure in processing chamber 201 within the range of, for example, 1 to 3990 Pa, and for example, 1000 Pa. The supply flow rate of Mo-containing gas controlled by MFC 312 is, for example, 0.1 to 1.0 slm, preferably within the range of 0.1 to 0.5 slm. The supply flow rates of Ar gas controlled by MFCs 512 and 522 are respectively set to, for example, within the range of 0.1 to 20 slm.

[0092] At this time, the gases flowing within the processing chamber 201 are only Mo-containing gas and Ar gas. Here, we will explain using MoO₂Cl₂ gas as the Mo-containing gas as an example. By supplying MoO₂Cl₂ gas as the Mo-containing gas, a Mo-containing layer is formed on the wafer 200 (the first Mo-containing film on the surface). The Mo-containing layer can be a Mo layer containing Cl and O, an adsorbed layer of MoO₂Cl₂, or both.

[0093] (Residual gas removal, step S22)

[0094] After the Mo-containing layer is formed, valve 314 is closed to stop the supply of Mo-containing gas.

[0095] Then, through the same processing steps as step S12 described above, unreacted gases or reaction byproducts that contribute to the formation of the Mo-containing layer and remain in the processing chamber 201 are removed from the processing chamber 201. That is, the processing chamber 201 is purged.

[0096] (Supply reducing gas, step S23)

[0097] After removing residual gas from processing chamber 201, valve 324 is opened to allow reducing gas to flow in gas supply pipe 320. The reducing gas flow rate is regulated by MFC 322, supplied to processing chamber 201 from gas supply port 420a of nozzle 420, and discharged from exhaust pipe 231. At this time, reducing gas is supplied to wafer 200. Simultaneously, valve 524 is opened to allow Ar gas to flow in gas supply pipe 520. The Ar gas flowing in gas supply pipe 520 is flow rate regulated by MFC 522. Ar gas is supplied to processing chamber 201 along with reducing gas and discharged from exhaust pipe 231. At this time, to prevent reducing gas from entering nozzle 410, valve 514 is opened to allow Ar gas to flow in gas supply pipe 510. Ar gas is supplied to processing chamber 201 via gas supply pipe 310 and nozzle 410 and discharged from exhaust pipe 231.

[0098] At this time, the APC valve 243 is adjusted to bring the pressure inside the processing chamber 201 to a range of, for example, 1 to 3990 Pa, and preferably 2000 Pa. The supply flow rate of the reducing gas controlled by the MFC 322 is, for example, 1 to 50 slm, preferably 15 to 30 slm. The supply flow rates of Ar gas controlled by the MFCs 512 and 522 are each set to a range of, for example, 0.1 to 30 slm. Here, when using H2 gas as the reducing gas, the time for supplying H2 gas to the wafer 200 is a second time shorter than the first time, i.e., a time within the range of 10 seconds to 5 minutes, for example, 1 minute. At this time, by setting the time for supplying H2 gas to the wafer 200 to 10 seconds or more, the reduction of Mo-containing gas adsorbed on the wafer 200 can be promoted, and by setting it to 5 minutes or less, productivity can be ensured.

[0099] At this point, the gases flowing within the processing chamber 201 are only H2 and Ar. The H2 gas undergoes a displacement reaction with at least a portion of the Mo-containing layer formed on the wafer 200 in step S21. That is, the O and Cl in the Mo-containing layer react with H2, detach from the Mo layer, and are discharged from the processing chamber 201 as reaction byproducts such as water vapor (H2O), hydrogen chloride (HCl), and chlorine (Cl2). Then, a Mo-containing layer that is substantially free of Cl and O is formed on the wafer 200.

[0100] Here, if the temperature of wafer 200 is set below 550°C, the reduction based on H2 gas supply in this step will be incomplete. Specifically, a film containing residual O, Cl, etc., from the Mo film will be formed. Furthermore, if the temperature of wafer 200 is set above 590°C, the reaction byproducts generated by the H2 gas supply in this step will hinder Mo adsorption, slowing down the film formation rate. Additionally, the resistivity of the film will increase.

[0101] That is, the temperature of wafer 200 is adjusted to a temperature range of 550°C to 590°C while supplying H2 gas as a reducing gas to wafer 200. By supplying H2 gas while maintaining the temperature of wafer 200 within this range, the reactivity is enhanced through H2 gas-based reduction. Therefore, Mo adsorption is promoted, and the film formation rate is accelerated. Furthermore, by supplying H2 gas while raising the temperature of wafer 200 to a temperature range of 550°C to 590°C, residual O, Cl, etc., in the first Mo-containing film are reduced, allowing for the removal of O, Cl, etc., from the first Mo-containing film and enabling the formation of a low-resistivity Mo-containing film.

[0102] (Residual gas removal, step S24)

[0103] After the Mo layer is formed, valve 324 is closed to stop the supply of reducing gas.

[0104] Then, through the same processing steps as step S14 described above, unreacted gases or reducing gases and reaction byproducts remaining in the processing chamber 201 that contribute to the formation of the Mo layer are removed from the processing chamber 201. That is, the processing chamber 201 is purged.

[0105] (Number of times specified)

[0106] By performing the above steps S21 to S24 in a loop at least once (a specified number of times (m times)), as follows: Figure 5 As shown in (C), a second Mo-containing film of a predetermined thickness (e.g., 10-20 nm) is formed on a wafer 200 on which a first Mo-containing film is formed. That is, a second Mo-containing film of a predetermined thickness is formed on the first Mo-containing film. The above cycle is preferably repeated multiple times. Furthermore, the second Mo-containing film formed in this process does not contact the AlO film of the substrate, and is formed on the first Mo-containing film that can suppress the diffusion of Al from the AlO film of the substrate. Therefore, the second Mo-containing film becomes a film that can suppress Al diffusion.

[0107] (Post-purging and atmospheric pressure recovery)

[0108] Ar gas is supplied into the processing chamber 201 through gas supply pipes 510 and 520, and exhaust gas is discharged through exhaust pipe 231. The Ar gas acts as a purging gas, thereby purging the processing chamber 201 with inert gas, removing residual gases and reaction byproducts from the processing chamber 201 (post-purging). Afterwards, the atmosphere in the processing chamber 201 is replaced with inert gas (inert gas replacement), and the pressure inside the processing chamber 201 is restored to atmospheric pressure (atmospheric pressure restoration).

[0109] (Wafer removal)

[0110] Next, the sealing cover 219 is lowered using the crystal boat lift 115, opening the lower end of the outer tube 203. Then, the processed wafer 200, supported by the crystal boat 217, is moved from the lower end of the outer tube 203 to the outside of the outer tube 203 (crystal boat unloading). Afterward, the processed wafer 200 is removed from the crystal boat 217 (wafer removal).

[0111] Here, in the first Mo-containing film formation process described above, the product of the wafer temperature (first temperature) and the reducing gas supply time (first time) is 450°C × 20 minutes = 9000°C / minute. Furthermore, in the second Mo-containing film formation process described above, the product of the wafer temperature (second temperature) and the reducing gas supply time (second time) is 580°C × 1 minute = 580°C / minute. That is, the temperature and time are set such that the product of the second temperature and the second time in the second Mo-containing film formation process is smaller than the product of the first temperature and the first time in the first Mo-containing film formation process. This allows for increased production capacity.

[0112] That is, in the substrate processing steps of this disclosure, a first Mo-containing film is formed on a wafer 200 on which an AlO film is formed, suppressing the diffusion of Al from the substrate AlO film, through a first Mo-containing film formation step. Then, in a second Mo-containing film formation step, a second Mo-containing film is formed on the wafer 200 on which the first Mo-containing film is formed, by increasing the temperature to enhance reactivity with the reducing gas, thereby forming a second Mo-containing film at a faster growth rate. In other words, a Mo-containing film composed of the first Mo-containing film and the second Mo-containing film is formed on the wafer 200 on which the AlO film is formed. Thus, a Mo-containing film that can suppress the diffusion of metal elements from the substrate metal film while improving productivity can be formed.

[0113] (3) Effects of this implementation method

[0114] According to this embodiment, one or more of the following effects can be obtained.

[0115] (a) It can suppress the diffusion of metal elements from the substrate metal film into the Mo-containing film and improve productivity.

[0116] (b) A second Mo-containing film can be formed on a first Mo-containing film with good surface roughness. That is, by forming a second Mo-containing film on a first Mo-containing film with flatness, the coverage can be improved. In other words, the embedding performance of the Mo-containing film used in the control gate electrode of the 3DNAND can be improved.

[0117] (c) It can form a Mo-containing film with reduced O, Cl, etc.

[0118] (d) It can form a Mo-containing film with low resistivity.

[0119] (4) Other implementation methods

[0120] The embodiments of this disclosure have been described in detail above. However, this disclosure is not limited to the embodiments described above, and various modifications can be made without departing from its spirit.

[0121] Figure 6This diagram illustrates a variation of the second Mo-containing film formation process described above. Specifically, during the first Mo-containing film formation process described above, a first Mo-containing film is formed on wafer 200. After heating the wafer, multiple second Mo-containing film formation processes are performed. Each time the cycle number of the second Mo-containing film formation process overlaps, the wafer temperature is increased while the supply time of the reducing gas in step S23 is shortened. Even in this case, the same as described above can be obtained. Figure 4 The substrate processing steps shown achieve the same effect.

[0122] Furthermore, in the above embodiments, the example of using MoO2Cl2 gas as the Mo-containing gas was described, but this disclosure is not limited thereto.

[0123] Furthermore, in the above embodiments, the case of using H2 gas as a reducing gas was described as an example, but this disclosure is not limited to this.

[0124] Furthermore, in the above embodiment, the pressure and temperature adjustment processes were described as an example before the second Mo-containing film formation process. However, the pressure and temperature adjustment processes can also be performed in parallel with a portion of the second Mo-containing film formation process. By doing so, the Mo-containing film can be formed during the pressure and temperature adjustment processes, increasing the film thickness. That is, there is a possibility of increasing manufacturing throughput. This method is particularly effective in single-sheet substrate processing apparatuses that process wafers 200 one by one. This is because in single-wafer substrate processing apparatuses, a temperature adjustment process is required for each wafer 200, reducing throughput.

[0125] Furthermore, in the above embodiments, an example of film formation using a batch vertical apparatus, i.e., a substrate processing apparatus, that processes multiple substrates at a time has been described. However, this disclosure is not limited to this and can also be appropriately applied to the case of film formation using a single-sheet substrate processing apparatus that processes one or more substrates at a time.

[0126] The following describes the embodiments, but this disclosure is not limited to these embodiments.

[0127] (5) Examples

[0128] (Example 1)

[0129] The production volume is compared between the case where a Mo-containing film is formed on a substrate using the substrate processing steps of this embodiment and the case where a Mo-containing film is formed on a substrate using the substrate processing steps of the comparative example.

[0130] In this embodiment, for the wafer 200 on which an AlO film is formed, the first Mo-containing film formation process described above is performed for 25 cycles at 450°C, and then the temperature is raised to 580°C to perform the second Mo-containing film formation process for 264 cycles, forming the film on the wafer 200 in two stages. The Mo-containing membrane is formed. The supply time of the reducing gas is set to 20 minutes in the first Mo-containing membrane formation process and 1 minute in the second Mo-containing membrane formation process.

[0131] In a comparative example, for a wafer 200 on which an AlO film is formed, the first Mo-containing film formation process described above is performed for 300 cycles at 450°C, thereby forming a film on the wafer 200. A thick Mo-containing membrane. The reducing gas is supplied for 20 minutes.

[0132] The production volume of forming a Mo-containing film on a wafer using the substrate processing steps of this embodiment is approximately three times that of forming a Mo-containing film on a wafer using the substrate processing steps of the comparative example.

[0133] That is, by forming a Mo-containing film on a wafer using the substrate processing steps of this embodiment, compared with forming a Mo-containing film on a wafer using the substrate processing steps of the comparative example, the production rate is more than three times higher, and the number of wafers processed per hour increases. In other words, a productivity improvement of more than three times is confirmed.

[0134] (Example 2)

[0135] Next, secondary ion mass spectrometry (SIMS) was used to analyze the depth-direction distribution of each element in the Mo-containing film formed by the substrate processing steps of this embodiment and the comparative example.

[0136] In a comparative example, for a wafer 200 on which an AlO film is formed, the first Mo-containing film formation process described above is performed for 250 cycles at 550°C to form a Mo-containing film on the wafer 200.

[0137] It was confirmed that the Mo-containing film formed on the wafer by the substrate processing steps of this embodiment suppressed the diffusion from the AlO film on the substrate.

[0138] In addition, it was confirmed that in the Mo-containing film formed on the wafer by the substrate processing process of the comparative example, Al diffuses into the vicinity of the surface of the Mo-containing film, and Cl and O, which hinder the adsorption of Mo, are also present.

[0139] That is, it was confirmed that the Mo-containing film formed by heating to 580°C after forming a Mo-containing film at 450°C as in the substrate processing procedure of this embodiment, compared with the Mo-containing film formed by heating at 550°C, suppressed the diffusion of Al from the AlO film on the substrate. It was confirmed that by forming a Mo-containing film on the AlO film on the substrate using the substrate processing procedure of this embodiment, the diffusion of Al from the AlO film on the substrate was suppressed.

[0140] (Example 3)

[0141] The intensity distribution of Al in the depth direction of Mo-containing films formed by heating the wafer 200 at temperatures of 450℃, 475℃, and 500℃ was compared.

[0142] As a result, it was confirmed that in the Mo-containing film formed by heating the wafer to 450°C, Al diffuses from the interface with the AlO film on the substrate to approximately 2.5 nm. Furthermore, it was confirmed that in the Mo-containing film formed by heating the wafer to 475°C, Al diffuses from the interface with the AlO film on the substrate to approximately 3 nm. Additionally, it was confirmed that in the Mo-containing film formed by heating the wafer to 500°C, Al diffuses from the interface with the AlO film on the substrate to approximately 5 nm. In other words, it was confirmed that by adjusting the wafer temperature and the thickness of the first Mo-containing film formed on the AlO film during the substrate processing, the diffusion of Al from the substrate AlO film within the Mo-containing film can be suppressed.

[0143] That is, it was confirmed that by adjusting the temperature of the heater 207 in the first Mo-containing film formation step of the above-mentioned substrate processing steps to a temperature within the range of 445°C or higher and 505°C or lower for the temperature of the wafer 200, a first Mo-containing film of a specified thickness can be formed, and diffusion from the AlO film on the substrate can be suppressed.

[0144] Symbol Explanation

[0145] 10 Substrate Processing Device

[0146] 121 controller

[0147] 200 wafers (substrate)

[0148] Processing Room 201.

Claims

1. A substrate processing method, characterized in that, The substrate processing method includes the following steps: (a1) Adjust the substrate to the first temperature; (a2) Supply the substrate with a molybdenum-containing gas containing molybdenum, oxygen, and chlorine; (a3) Supply the substrate with a reducing gas for a first time; (a4) After (a1), by performing (a2) and (a3) ​​more than once, a first molybdenum-containing film containing oxygen and chlorine is formed on the substrate; (b1) After (a4), while the reducing gas is supplied to the substrate and the molybdenum-containing gas is not supplied to the substrate, the oxygen and chlorine are removed from the first molybdenum-containing film while the substrate is adjusted to a second temperature; (b2) Supply the molybdenum-containing gas to the substrate; (b3) Supply the reducing gas to the substrate at a second time; as well as (b4) Following (b1), a second molybdenum-containing film is formed on the first molybdenum-containing film by performing (b2) and (b3) more than once. The first temperature is above 445°C and below 505°C. The second temperature is above 550°C and below 590°C.

2. The substrate processing method according to claim 1, characterized in that, The second time is shorter than the first time.

3. The substrate processing method according to claim 1, characterized in that, The first time period is between 10 minutes and 30 minutes. The second time is more than 10 seconds and less than 5 minutes.

4. The substrate processing method according to claim 1, characterized in that, The first temperature, the second temperature, the first time, and the second time are set in such a way that the product of the second temperature and the second time is less than the product of the first temperature and the first time.

5. The substrate processing method according to claim 1, characterized in that, The experiment was conducted in an inert gas atmosphere (b1).

6. The substrate processing method according to claim 5, characterized in that, The inert gas is a rare gas.

7. The substrate processing method according to claim 6, characterized in that, The rare gas is argon.

8. The substrate processing method according to claim 1, characterized in that, The reducing gas is a hydrogen-containing gas.

9. The substrate processing method according to claim 8, characterized in that, The hydrogen-containing gas is hydrogen.

10. The substrate processing method according to claim 1, characterized in that, (b1) is performed at a pressure higher than that in (a4) and (b4).

11. The substrate processing method according to claim 1, characterized in that, In (b1), during the process of adjusting to the second temperature, (b2) and (b3) are performed more than once.

12. The substrate processing method according to claim 1, characterized in that, In (a4), the first molybdenum-containing film is formed on a substrate on which an AlO film is formed.

13. The substrate processing method according to claim 1, characterized in that, In (a4), as the substrate, a first molybdenum-containing film with an average roughness Ra of less than 1.0 nm is formed on a substrate on which an AlO film is formed on the surface.

14. The substrate processing method according to claim 1, characterized in that, In (b4), the second molybdenum-containing membrane is formed while the oxygen and chlorine are removed from the first molybdenum-containing membrane.

15. The substrate processing method according to claim 1, characterized in that, In (a2), the molybdenum-containing gas is supplied from a molybdenum-containing gas supply system. In (a3), rare gas is supplied from the molybdenum-containing gas supply system to the processing chamber.

16. The substrate processing method according to claim 15, characterized in that, In (a3), the reducing gas is supplied from the reducing gas supply system. In (a2), rare gas is supplied from the reducing gas supply system to the processing chamber.

17. The substrate processing method according to claim 1, characterized in that, In (b4), a barrier film or control electrode film having the first molybdenum-containing film and the second molybdenum-containing film is formed.

18. A method for manufacturing a semiconductor device, characterized in that, The manufacturing method comprises the following steps: (a1) Adjust the substrate to the first temperature; (a2) Supply the substrate with a molybdenum-containing gas containing molybdenum, oxygen, and chlorine; (a3) Supply the substrate with a reducing gas for a first time; (a4) After (a1), by performing (a2) and (a3) ​​more than once, a first molybdenum-containing film containing oxygen and chlorine is formed on the substrate; (b1) After (a4), while the reducing gas is supplied to the substrate and the molybdenum-containing gas is not supplied to the substrate, the oxygen and chlorine are removed from the first molybdenum-containing film while the substrate is adjusted to a second temperature; (b2) Supply the molybdenum-containing gas to the substrate; (b3) Supply the reducing gas to the substrate at a second time; as well as (b4) Following (b1), a second molybdenum-containing film is formed on the first molybdenum-containing film by performing (b2) and (b3) more than once. The first temperature is above 445°C and below 505°C. The second temperature is above 550°C and below 590°C.

19. A computer-readable recording medium, characterized in that, Its records contain a program that uses a computer to cause the substrate processing apparatus to perform the following steps: (a1) Adjust the substrate to the first temperature; (a2) Supply the substrate with a molybdenum-containing gas containing molybdenum, oxygen, and chlorine; (a3) Supply the substrate with a reducing gas for a first time; (a4) After (a1), by performing (a2) and (a3) ​​more than once, a first molybdenum-containing film containing oxygen and chlorine is formed on the substrate; (b1) After (a4), while the reducing gas is supplied to the substrate and the molybdenum-containing gas is not supplied to the substrate, the oxygen and chlorine are removed from the first molybdenum-containing film while the substrate is adjusted to a second temperature; (b2) Supply the molybdenum-containing gas to the substrate; (b3) Supply the reducing gas to the substrate at a second time; as well as (b4) Following (b1), a second molybdenum-containing film is formed on the first molybdenum-containing film by performing (b2) and (b3) more than once. The first temperature is above 445°C and below 505°C. The second temperature is above 550°C and below 590°C.

20. A substrate processing apparatus, characterized in that, have: The heating system regulates the temperature of the substrate. A molybdenum-containing gas supply system that supplies a molybdenum-containing gas containing molybdenum, oxygen, and chlorine to the substrate; A reducing gas supply system that supplies reducing gas to the substrate; as well as The control unit is configured to control the heating system, the molybdenum-containing gas supply system, and the reducing gas supply system to perform the following processes: (a1) Adjust the substrate to a first temperature; (a2) Supply the substrate with the molybdenum-containing gas containing molybdenum, oxygen, and chlorine; (a3) Supply the reducing gas to the substrate at a first time; (a4) After (a1), by performing (a2) and (a3) ​​more than once, a first molybdenum-containing film containing oxygen and chlorine is formed on the substrate; (b1) After (a4), while the reducing gas is supplied to the substrate and the molybdenum-containing gas is not supplied to the substrate, the oxygen and chlorine are removed from the first molybdenum-containing film while the substrate is adjusted to a second temperature; (b2) Supply the molybdenum-containing gas to the substrate; (b3) Supply the reducing gas to the substrate at a second time; as well as (b4) Following (b1), a second molybdenum-containing film is formed on the first molybdenum-containing film by performing (b2) and (b3) more than once. The first temperature is above 445°C and below 505°C. The second temperature is above 550°C and below 590°C.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor device and substrate processing apparatus

    JP2011066263A

  • Manufacturing method of semiconductor device, substrate processing device, and program

    WO2019058608A1

  • Electrode of semiconductor element and method for forming the same

    JP2003309084A

  • KR20190024806A