Trimetallic catalyst made of nickel, molybdenum and tungsten and its use in hydrotreating and / or hydrocracking processes

By optimizing the ratio of nickel, molybdenum, tungsten and phosphorus and the addition of organic compounds, the activity and stability of the hydrotreatment catalyst is improved, and the shortcomings of existing catalysts in improving fuel quality are solved, and more efficient hydrotreatment is achieved Effect.

CN115996796BActive Publication Date: 2024-11-19IFP ENERGIES NOUVELLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180046431.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-29
Filing Date
2021-06-18
Publication Date
2024-11-19
Estimated Expiration
2041-06-18

AI Technical Summary

Technical Problem

The performance quality of existing hydrotreatment catalysts in improving the sulfur content, nitrogen content and aromatic content of diesel fuels remains insufficient and the production is complex, resulting in challenges in industrial deployment.

Method used

Using a catalyst composed of nickel, molybdenum and tungsten based on alumina or silica support, by optimizing the ratio of metal to phosphorus, especially the molar ratios of WO3/MoO3, NiO/(WO3+MoO3 and P2O5/(WO3+MoO3+MoO3, Combined with the addition of organic compounds, the activity of the catalyst is enhanced.

Benefits of technology

The hydrotreating activity of the catalyst is significantly improved, especially in the hydrogenation reaction of aromatic hydrocarbons, the temperature at which the target sulfur content and aromatic hydrocarbon content is reduced, the circulation time is extended, and the stability of the catalyst is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004026491550000061
    Figure BDA0004026491550000061
  • Figure BDA0004026491550000071
    Figure BDA0004026491550000071
  • Figure BDA0004026491550000231
    Figure BDA0004026491550000231
Patent Text Reader

Abstract

A subject of the invention is a catalyst comprising a support and an active phase consisting of nickel, molybdenum and tungsten, and phosphorus, wherein the nickel content measured in the form of NiO is between 3% and 4% by weight, relative to the total weight of the catalyst; the molybdenum content measured in the form of MoO3 is between 2% and 4% by weight; the tungsten content measured in the form of WO3 is between 34% and 40% by weight; the phosphorus content measured in the form of P2O5 is between 3% and 4% by weight; the WO3 / MoO3 molar ratio is between 5.3 and 12.4 mol / mol, the NiO / (WO3+MoO3) molar ratio is between 0.20 and 0.33 mol / mol, and the P2O5 / (WO3+MoO3) molar ratio is between 0.21 and 0.34 mol / mol. The invention also relates to a process for its preparation and its use in hydrotreatment and / or hydrocracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a trimetallic catalyst based on nickel, molybdenum and tungsten, a process for its preparation and its use in the field of hydrotreatment and / or hydrocracking.

[0002] Conventional hydroprocessing catalysts generally comprise an oxide support and an active phase based on metals from groups VIb and VIII in the form of their oxides and phosphorus. The preparation of these catalysts generally comprises a stage of impregnation of the metals and phosphorus on the support, followed by drying and calcination, so as to obtain the active phase in the form of its oxide. Before using them in hydroprocessing and / or hydrocracking reactions, these catalysts are generally sulfided to form active entities.

[0003] Those skilled in the art have recommended the addition of organic compounds to hydroprocessing catalysts to improve the activity of the catalyst, particularly for catalysts that have been prepared by impregnation followed by drying but not subsequent calcination. These catalysts are often referred to as "additive-impregnated dry catalysts".

[0004] In general, the purpose of the catalysts used for the hydrotreatment of hydrocarbon fractions is to remove the sulfur-based compounds, nitrogen-based compounds or aromatic compounds contained therein, in order, for example, to produce a petroleum product meeting the specifications (sulfur content, aromatics content, etc.) required for a given application (motor vehicle fuel, gasoline or gas oil, heating oil, aviation fuel).

[0005] As legislation regarding air quality is tightened in many countries, efforts are ongoing to develop more efficient catalysts and processes for the production of low-sulfur fuels, especially diesel. Although great progress has been made in the development of efficient catalysts for these processes, major challenges remain, such as their mild saturation activity towards aromatic hydrocarbons. As recent environmental restrictions have set minimum values ​​for the cetane number and lower limits for the content of polycyclic aromatic hydrocarbons in the diesel fraction, improving the aromatic saturation activity of hydroprocessing catalysts has become a research focus.

[0006] Trimetallic catalysts based on nickel, molybdenum and tungsten are known to increase not only hydrodesulfurization (HDS) and hydrodenitrogenation (HDN), but also hydrogenation of aromatics (HDA).

[0007] For example, there are documents describing bulk NiMoW trimetallic catalysts with low binder content (US 6 162350, US 6 299 760, WO00 / 41810, US 6 566 296 or even US2017 / 015644). These catalysts, also known as "bulk" catalysts, do not contain a support. Although these catalysts show high activity in hydroprocessing, they show the disadvantages of being very expensive (high metal content) and non-renewable.

[0008] The prior art also mentions supported NiMoW trimetallic catalysts, such as those described by Solmanov et al. in the publication Russian Journal of Applied Chemistry (2018, Vol. 91, No. 8, pp. 1363-1369).

[0009] Document US2019 / 126254 describes a supported NiMoWP catalyst containing 15 to 25 wt. % (expressed as oxide) of Mo and / or W, 3 to 6 wt. % (expressed as oxide) of Ni, 0.1 to 1 wt. % (expressed as oxide) of P and 0.1 to 0.7 mol % of additives, relative to the metal (VIb + VIII).

[0010] Document US 8 697 598 discloses a supported NiMoW catalyst containing phosphorus and / or fluorine, wherein the nickel content is 1 wt % to 10 wt % (expressed as NiO), the total content of molybdenum and tungsten is 10 wt % to 50 wt % (expressed as oxides), the content of fluorine and / or phosphorus (expressed as elements) is 0.2 wt % to 14 wt %, and the WO3 / Mo3 molar ratio is 2.6 to 30.

[0011] Regardless of the catalyst chosen, the modifications induced do not always sufficiently improve the performance qualities of the catalyst to meet the specifications regarding the sulfur, nitrogen and / or aromatics content of the fuel. Furthermore, since these methods are complex to implement, their deployment in industry is often very complicated.

[0012] Therefore, it is of vital importance for catalyst manufacturers to find new hydrotreating and / or hydrocracking catalysts with improved performance qualities.

[0013] Overview

[0014] The invention relates to a catalyst comprising a support based on aluminum oxide or silicon dioxide or silicon dioxide-alumina, an active phase consisting of nickel, molybdenum and tungsten, and phosphorus, characterized in that:

[0015] - a nickel content of 3 to 4% by weight, measured in the form of NiO, relative to the total weight of the catalyst,

[0016] - a molybdenum content of 2% to 4% by weight, measured in the form of MoO3, relative to the total weight of the catalyst,

[0017] - a tungsten content, measured in the form of WO3, of 34% to 40% by weight, relative to the total weight of the catalyst,

[0018] - a phosphorus content of 3% to 4% by weight, measured in the form of P2O5, relative to the total weight of the catalyst,

[0019] -WO3 / MoO3 molar ratio is 5.3 to 12.4 mol / mol,

[0020] -NiO / (WO3+MoO3) molar ratio is 0.20 to 0.33 mol / mol,

[0021] -P2O5 / (WO3+MoO3) molar ratio is 0.21 to 0.34 mol / mol.

[0022] The Applicant Company has found that, surprisingly, a catalyst based on an active phase consisting of nickel, molybdenum and tungsten in the presence of phosphorus deposited on a support and exhibiting a specific ratio between these different metals and / or phosphorus, exhibits, by synergistic effects, a better hydroprocessing activity, in particular in the hydrogenation of aromatics (HDA), but also in hydrodesulfurization (HDS) and / or hydrodenitrogenation (HDN), compared to the catalysts disclosed in the prior art. Typically, by virtue of the increase in activity, the temperature required to reach the desired sulfur content, nitrogen content or aromatics content (e.g., in the ULSD or Ultra Low Sulfur Diesel mode, up to 10 ppm of sulfur in the case of gas oil feedstocks, or a content of <8% by weight of polyaromatics and a cetane number of >46 (summer) and a cetane number of 43 to 46 (winter)) can be reduced. Similarly, the stability is improved due to the extension of the cycle time by the necessary temperature reduction.

[0023] Without wishing to be bound by any one theory, optimizing the content of each metal and phosphorus using specific ratios will enable obtaining an active phase that brings improved catalytic performance qualities. This is because tungsten is known to be more active than molybdenum in the hydrogenation of aromatics; however, its sulfidation is more difficult. An increase in the proximity of molybdenum in the tungsten-containing active phase and the WO3 / MoO3 ratio can improve the sulfidability of tungsten and the observed catalytic performance qualities until a certain WO3 / MoO3 ratio is reached, when the molybdenum content is too low to affect the sulfidability of tungsten. Therefore, the optimization of the WO3 / MoO3 ratio, combined with the optimized NiO / (WO3+MoO3) and P2O5 / (WO3+MoO3) ratios, can obtain a catalyst that is very active in hydroprocessing, especially in the hydrogenation of aromatics (HDA).

[0024] According to an alternative form, the catalyst is characterized in that:

[0025] - a nickel content of 3.1% to 3.9% by weight, measured in the form of NiO, relative to the total weight of the catalyst,

[0026] - a molybdenum content, measured in the form of MoO3, of 2.2% to 3.8% by weight, relative to the total weight of the catalyst,

[0027] - a tungsten content, measured in the form of WO3, of 35% to 39.9% by weight relative to the total weight of the catalyst,

[0028] - a phosphorus content of 3.1% to 3.9% by weight, measured in the form of P2O5, relative to the total weight of the catalyst,

[0029] -WO3 / MoO3 molar ratio is 5.7 to 11.1 mol / mol,

[0030] -NiO / (WO3+MoO3) molar ratio is 0.21 to 0.31 mol / mol,

[0031] -P2O5 / (WO3+MoO3) molar ratio is 0.22 to 0.33 mol / mol.

[0032] According to an alternative form, the catalyst is characterized in that:

[0033] - a nickel content of 3.2% to 3.8% by weight, measured in the form of NiO, relative to the total weight of the catalyst,

[0034] - a molybdenum content, measured in the form of MoO3, of 2.5% to 3.5% by weight, relative to the total weight of the catalyst,

[0035] - a tungsten content, measured in the form of WO3, of 36% to 39% by weight relative to the total weight of the catalyst,

[0036] - a phosphorus content of 3.2% to 3.8% by weight, measured in the form of P2O5, relative to the total weight of the catalyst,

[0037] -WO3 / MoO3 molar ratio is 6.4 to 9.7 mol / mol,

[0038] -NiO / (WO3+MoO3) molar ratio is 0.22 to 0.30 mol / mol,

[0039] -P2O5 / (WO3+MoO3) molar ratio is 0.23 to 0.32 mol / mol.

[0040] According to one alternative form, the catalyst exhibits a density of metal from group VIb, expressed as the number of atoms of said metal per unit area of ​​catalyst, of from 5 to 12 atoms of metal from group VIb / nm 2 catalyst.

[0041] According to one alternative form, the catalyst additionally comprises an organic compound containing oxygen and / or nitrogen and / or sulphur.

[0042] According to this alternative form, the organic compound is chosen from compounds containing one or more chemical functional groups, or compounds containing a furan ring, or sugars, and the chemical functional groups are chosen from carboxyl, alcohol, thiol, thioether, sulfone, sulfoxide, ether, aldehyde, ketone, ester, carbonate, amine, nitrile, imide, oxime, urea or amide functional groups.

[0043] According to an alternative form, the organic compound is chosen from γ-valerolactone, 2-acetylbutyrolactone, triethylene glycol, diethylene glycol, ethylene glycol, ethylenediaminetetraacetic acid (EDTA), maleic acid, malonic acid, citric acid, acetic acid, gluconic acid, glucose, fructose, sucrose, sorbitol, xylitol, γ-ketovaleric acid, di(C1-C4 alkyl) succinates and more particularly dimethyl succinate, dimethylformamide, 1-methyl-2-pyrrolidone, propylene carbonate, 2-methoxyethyl 3-oxobutyrate, N,N-dihydroxyethylglycine (bicine), N-tris(hydroxymethyl)methylglycine (tricine), 2-furaldehyde (furfural) (also known as furfural), 5-hydroxymethylfuraldehyde (also known as 5-(hydroxymethyl)-2-furoxaldehyde furanaldehyde or 5-HMF), 2-acetylfuran, 5-methyl-2-furanaldehyde, ascorbic acid, butyl lactate, ethyl lactate, butyl butyrolactate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, 2-ethoxyethyl acetate, 2-butoxyethyl acetate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 1,5-pentanediol, 1 -(2-hydroxyethyl)-2-pyrrolidone, 1-(2-hydroxyethyl)-2,5-pyrrolidinedione, 5-methyl-2(3H)-furanone, 1-methyl-2-piperidone, 4-aminobutyric acid, butyl glycolate, ethyl 2-mercaptopropionate, ethyl 4-oxopentanoate, diethyl maleate, dimethyl maleate, dimethyl fumarate, diethyl fumarate, dimethyl adipate and dimethyl 3-oxoglutarate.

[0044] According to an alternative form, the content of said organic compound is from 1% to 30% by weight relative to the total weight of said catalyst.

[0045] According to one alternative form, the catalyst is at least partially sulphurized.

[0046] The invention also relates to a process for preparing the catalyst according to the invention, said process comprising the following stages:

[0047] a) contacting at least one nickel precursor, at least one molybdenum precursor and at least one tungsten precursor and phosphorus with a support based on alumina or silica or silica-alumina in order to obtain a catalyst precursor,

[0048] b) drying the catalyst precursor obtained from stage a) at a temperature below 200°C.

[0049] According to one alternative form, the preparation process additionally comprises a stage c) in which the catalyst obtained in stage b) is calcined at a temperature ranging from 200°C to 550°C.

[0050] According to one alternative form, the preparation process additionally comprises a stage d) in which the catalyst obtained in stage b) or in stage c) is sulphurized.

[0051] The invention also relates to the use of the catalyst according to the invention in a process for the hydrotreatment and / or hydrocracking of hydrocarbon fractions. DETAILED DESCRIPTION OF THE INVENTION

[0053] definition

[0054] In the following, the families of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, published by CRC Press, edited by DRLide, the 81st edition, 2000-2001). For example, family VIII according to the CAS classification corresponds to metals in columns 8, 9 and 10 according to the new IUPAC classification.

[0055] The term "specific surface area" is understood to mean the BET specific surface area (S) determined by nitrogen adsorption according to standard ASTM D 3663-78 established by the Brunauer-Emmett-Teller method described in the journal "The journal of The American Chemical Societ (1938, 60, 309)". BET , unit: m 2 / g).

[0056] The total pore volume of the catalyst or of the support used to prepare the catalyst is understood to mean the volume measured by mercury intrusion porosimetry according to standard ASTM D4284-83, at a maximum pressure of 4000 bar (400 MPa), using a surface tension of 484 dynes / cm and a contact angle of 140°. A wetting angle equal to 140° is assumed, following the advice of pages 1050-1055 of the publication “Techniques de l'ingénieur, traité Analysis et caractérisation” [Techniques of the Engineer, Analysis and Characterization Treatise], written by Jean Charpin and Bernard Rasneur. For greater accuracy, the value of the total pore volume corresponds to the total pore volume measured by mercury intrusion porosimetry on a sample minus the value of the total pore volume measured by mercury intrusion porosimetry on the same sample at a pressure corresponding to 30 psi (about 0.2 MPa).

[0057] The contents of metals from Groups VIII and VIb and of phosphorus were measured by X-ray fluorescence.

[0058] The content of metals from group VIb, metals from group VIII and phosphorus in the catalyst is expressed as oxides after correction for the loss on ignition of a sample of the catalyst burnt out in a muffle furnace at 550° C. for two hours. The loss on ignition is due to the loss of water. It is determined according to ASTM D7348.

[0059] Hydrotreatment is understood to mean reactions which include in particular hydrodesulfurization (HDS), hydrodenitrogenation (HDN) and hydrogenation of aromatics (HDA).

[0060] catalyst

[0061] The invention relates to a catalyst comprising a support based on aluminum oxide or silicon dioxide or silicon dioxide-alumina, an active phase consisting of nickel, molybdenum and tungsten, and phosphorus, characterized in that:

[0062] - a nickel content of 3 to 4% by weight, measured in the form of NiO, relative to the total weight of the catalyst,

[0063] - a molybdenum content of 2% to 4% by weight, measured in the form of MoO3, relative to the total weight of the catalyst,

[0064] - a tungsten content, measured in the form of WO3, of 34% to 40% by weight, relative to the total weight of the catalyst,

[0065] - a phosphorus content of 3% to 4% by weight, measured in the form of P2O5, relative to the total weight of the catalyst,

[0066] -WO3 / MoO3 molar ratio is 5.3 to 12.4 mol / mol,

[0067] -NiO / (WO3+MoO3) molar ratio is 0.20 to 0.33 mol / mol,

[0068] -P2O5 / (WO3+MoO3) molar ratio is 0.21 to 0.34 mol / mol.

[0069] The hydrogenation function of the catalyst, also known as the active phase, is composed of nickel, molybdenum and tungsten.

[0070] The nickel content, measured as NiO, is from 3% to 4% by weight, preferably from 3.1% to 3.9% by weight and more preferably from 3.2% to 3.8% by weight, relative to the total weight of the catalyst.

[0071] The molybdenum content, measured in the form of MoO3, is from 2% to 4% by weight, preferably from 2.2% to 3.8% by weight and more preferably from 2.5% to 3.5% by weight, relative to the total weight of the catalyst.

[0072] The tungsten content, measured as WO3, is from 34% to 40% by weight, preferably from 35% to 39.9% by weight and more preferably from 36% to 39% by weight, relative to the total weight of the catalyst.

[0073] The WO3 / MoO3 molar ratio is 5.3 to 12.4 mol / mol, preferably 5.7 to 11.1 mol / mol, and more preferably 6.4 to 9.7 mol / mol.

[0074] The NiO / (WO3+MoO3) molar ratio is 0.20 to 0.33 mol / mol, preferably 0.21 to 0.31 mol / mol, and even more preferably 0.22 to 0.30 mol / mol.

[0075] The catalyst according to the invention also contains phosphorus as a dopant. A dopant is an added element which does not exhibit any catalytic properties itself, but which increases the catalytic activity of the active phase.

[0076] The phosphorus content, measured as P2O5, relative to the total weight of the catalyst, is preferably from 3 to 4% by weight, preferably from 3.1 to 3.9% by weight and very preferably from 3.2 to 3.8% by weight.

[0077] The P2O5 / (WO3+MoO3) molar ratio is 0.21 to 0.34 mol / mol, preferably 0.22 to 0.33 mol / mol, and even more preferably 0.23 to 0.32 mol / mol.

[0078] Furthermore, the catalyst exhibits a metal from Group VIb (Mo+W) density expressed as the number of atoms of said metal per unit area of ​​catalyst of 5 to 12, preferably 6 to 11, even more preferably 7 to 10 metal atoms from Group VIb / nm 2 The density of the metal from Group VIb is expressed as the number of atoms of the metal from Group VIb per unit area of ​​the catalyst (number of atoms of the metal from Group VIb / nm 2 Catalyst) is expressed, for example, by the following relationship:

[0079]

[0080] in:

[0081] X Mo = weight % of molybdenum;

[0082] X W = weight % of tungsten;

[0083] N A = Avogadro's number, equal to 6.022×10 23 ;

[0084] S = specific surface area of ​​the catalyst (m 2 / g), measured according to standard ASTM D3663;

[0085] M Mo = molar mass of molybdenum;

[0086] M W = molar mass of tungsten.

[0087] For example, if the catalyst contains 3 wt% molybdenum oxide MoO3 (i.e. 2.0 wt% Mo) and 29.3 wt% tungsten oxide, and has a molecular weight of 122 m 2 / g specific surface area, then the density d(Mo+W) is equal to:

[0088]

[0089] The catalyst according to the invention may also advantageously comprise at least one dopant chosen from boron, fluorine and mixtures of boron and fluorine.

[0090] When the catalyst contains boron or fluorine or a mixture of boron and fluorine, the content of boron or fluorine or the content of the mixture of the two, expressed as boron oxide and / or fluorine, is preferably from 0.1 to 10% by weight, preferably from 0.2 to 7% by weight and very preferably from 0.2 to 5% by weight, relative to the total weight of the catalyst.

[0091] The pore volume of the catalyst is usually 0.1 cm 3 / g to 1.5cm 3 / g, preferably 0.15cm 3 / g to 1.1cm 3 / g. The total pore volume is measured by mercury intrusion according to standard ASTM D4284, using a wetting angle of 140°, as described in the work "Adsorption by Powders & Porous Solids: Principle, Methodology and Applications (Academic Press, 1999)" by Rouquerol F., Rouquerol J. and Singh K., for example by Micromeritics TM Brand Autopore III TM Type equipment.

[0092] The catalyst is characterized by 5 to 350 m 2 / g, preferably 10 to 330m 2 / g, preferably 40 to 320m 2 / g, very preferably 50 to 300m 2 In the present invention, the specific surface area is determined by the BET method according to standard ASTM D3663, which is described in the same work mentioned above.

[0093] The support of the catalyst comprises, and preferably consists of, alumina or silica or silica-alumina.

[0094] When the support of the catalyst is based on alumina, it contains more than 50% by weight of alumina relative to the total weight of the support and generally it contains only alumina or silica-alumina as described below.

[0095] Preferably, the support comprises alumina, and preferably extruded alumina.Preferably, the alumina is gamma-alumina.

[0096] The alumina support advantageously exhibits a 0.1 to 1.5 cm 3 / g, preferably 0.4 to 1.1 cm 3The total pore volume is measured by mercury intrusion according to standard ASTM D4284, using a wetting angle of 140°, as described in the work "Adsorption by Powders & Porous Solids: Principle, Methodology and Applications (Academic Press, 1999)" by Rouquerol F., Rouquerol J. and Singh K., for example by Micromeritics TM Brand Autopore III TM Type equipment.

[0097] The specific surface area of ​​the alumina support is advantageously between 5 and 400 m 2 / g, preferably 10 to 350m 2 / g, more preferably 40 to 350m 2 In the present invention, the specific surface area is determined by the BET method according to standard ASTM D3663, which is described in the same work mentioned above.

[0098] In another preferred embodiment, the support of the catalyst is silica-alumina, which contains at least 50% by weight of alumina relative to the total weight of the support. The silica content in the support is at most 50% by weight, generally less than or equal to 45% by weight, preferably less than or equal to 40% by weight, relative to the total weight of the support.

[0099] Sources of silicon are well known to those skilled in the art. Mention may be made, by way of example, of silicic acid, silicon dioxide in powder form or in colloidal form (silica sol), or tetraethyl orthosilicate Si(OEt)4.

[0100] When the support of the catalyst is based on silica, it contains more than 50% by weight of silica relative to the total weight of the support and generally contains only silica.

[0101] According to a particularly preferred alternative form, the support consists of alumina, silica or silica-alumina.

[0102] In addition, the carrier can also advantageously comprise a zeolite. In this case, any zeolite source known to those skilled in the art and any relevant preparation method can be adopted. Preferably, the zeolite is selected from FAU, BEA, ISV, IWR, IWW, MEI, UWY, and preferably the zeolite is selected from FAU and BEA, such as Y zeolite and / or beta zeolite, and particularly preferably, such as USY zeolite and / or beta zeolite. When zeolite is present, its content is 0.1 wt % to 50 wt % relative to the gross weight of the carrier.

[0103] The support is advantageously provided in the form of beads, extrudates, granules or irregular and non-spherical agglomerates, the specific shape of which may result from a comminution stage.

[0104] The catalyst according to the invention may additionally contain an organic compound or group of organic compounds, which are known to be used as additives. The effect of the additive is to increase the catalytic activity compared to a catalyst not impregnated with an additive. More specifically, the catalyst according to the invention may additionally contain one or more oxygen-containing organic compounds and / or one or more nitrogen-containing organic compounds and / or one or more sulfur-containing organic compounds. Preferably, the catalyst according to the invention may additionally contain one or more oxygen-containing organic compounds and / or one or more nitrogen-containing organic compounds. Preferably, the organic compound contains at least two carbon atoms and at least one oxygen and / or nitrogen atom, and does not contain other heteroatoms.

[0105] Typically, the organic compound is chosen from compounds comprising one or more chemical functional groups, or compounds containing a furan ring, or sugars, wherein the chemical functional groups are chosen from carboxyl, alcohol, thiol, thioether, sulfone, sulfoxide, ether, aldehyde, ketone, ester, carbonate, amine, nitrile, imide, oxime, urea or amide functional groups.

[0106] The oxygen-containing organic compound can be one or more selected from compounds containing one or more chemical functional groups, or compounds containing furan rings, or sugars, and the chemical functional groups are selected from carboxyl, alcohol, ether, aldehyde, ketone, ester or carbonate functional groups. The oxygen-containing organic compound is understood herein to refer to a compound that does not contain another heteroatom. For example, the oxygen-containing organic compound can be selected from one or more of the following: ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol (molecular weight 200 to 1500g / mol), propylene glycol, 2-butoxyethanol, 2-(2-butoxyethoxy)ethanol, 2-(2-methoxyethoxy)ethanol, triethylene glycol dimethyl ether, glycerol, acetophenone, 2,4-pentanedione, pentanone, acetic acid, oxalic acid, maleic acid, malic acid, malonic acid, oxalic acid, gluconic acid, tartaric acid, citric acid, gamma-glucose ...citric acid, gamma-glucose, citric acid, gamma-glucose, citric acid, gamma- -ketovaleric acid, di(C1-C4-alkyl) succinates, and more particularly dimethyl succinate, methyl acetoacetate, ethyl acetoacetate, 2-methoxyethyl 3-oxobutyrate, 2-methacryloyloxyethyl 3-oxobutyrate, dibenzofuran, crown ethers, phthalic acid, glucose, fructose, sucrose, sorbitol, xylitol, γ-valerolactone, 2-acetylbutyrolactone, propylene carbonate, 2-furfural (also known as furfural), 5-hydroxymethylfurfural (also known as 5-(hydroxymethyl)-2-furan formaldehyde or 5-HMF), 2-acetylfuran, 5-methyl-2-furfurylcarboxaldehyde, methyl 2-furoate, furfuryl alcohol (also known as furfuryl alcohol), furfuryl acetate, ascorbic acid, butyl lactate, ethyl lactate, butyl butyrolactate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, 2-ethoxyethyl acetate, 2-butoxyethyl acetate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,5 -hexanediol, 3-ethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 5-methyl-2(3H)-furanone, butyl glycolate, ethyl 4-oxopentanoate, diethyl maleate, dimethyl maleate, dimethyl fumarate, diethyl fumarate, dimethyl adipate, dimethyl 3-oxoglutarate, dimethyl tartrate, diethyl tartrate, diisopropyl tartrate, di-tert-butyl tartrate, dimethyl malate, diethyl malate, diisopropyl malate and dibutyl malate.

[0107] The nitrogen-containing organic compound can be one or more selected from compounds containing one or more chemical functional groups selected from amine or nitrile functional groups. Nitrogen-containing organic compounds are understood herein to mean compounds that do not contain another heteroatom. For example, the nitrogen-containing organic compound can be one or more selected from ethylenediamine, diethylenetriamine, hexamethylenediamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, acetonitrile, octylamine, guanidine and carbazole.

[0108] The oxygen-containing organic compound and the nitrogen-containing organic compound may be one or more selected from compounds containing one or more chemical functional groups selected from carboxylic acid, alcohol, ether, aldehyde, ketone, ester, carbonate, amine, nitrile, imide, amide, urea or oxime functional groups. The oxygen-containing organic compound and the nitrogen-containing organic compound are understood herein to mean a compound that does not contain another heteroatom. For example, the oxygen-containing organic compound and the nitrogen-containing organic compound may be one or more selected from the following: 1,2-cyclohexanediaminetetraacetic acid, monoethanolamine (MEA), 1-methyl-2-pyrrolidone, dimethylformamide, ethylenediaminetetraacetic acid (EDTA), alanine, glycine, nitrilotriacetic acid (NTA), N-(2-hydroxyethyl)ethylenediamine-N,N′,N′-triacetic acid (HEDTA), diethylenetriaminepentaacetic acid (DTPA), tetramethylurea, glutamic acid, di Methylglyoxime, N,N-dihydroxyethylglycine, N-tris(hydroxymethyl)methylglycine, 2-methoxyethyl cyanoacetate, 1-ethyl-2-pyrrolidone, 1-vinyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 1-(2-hydroxyethyl)-2-pyrrolidone, 1-(2-hydroxyethyl)-2,5-pyrrolidinedione, 1-methyl-2-piperidone, 1-acetyl-2-azacycloheptanone, 1-vinyl-2-azacycloheptanone and 4-aminobutyric acid.

[0109] The sulfur-containing organic compound may be one or more selected from compounds containing one or more chemical functional groups selected from thiol, thioether, sulfone or sulfoxide functional groups. For example, the sulfur-containing organic compound may be one or more selected from the following: thioglycolic acid, 2,2'-thiodiethanol, 2-hydroxy-4-methylthiobutyric acid, sulfone derivatives of benzothiophene or sulfoxide derivatives of benzothiophene, ethyl 2-mercaptopropionate, methyl 3-(methylthio)propionate and ethyl 3-(methylthio)propionate.

[0110] Preferably, the organic compound comprises oxygen; preferably, it is selected from γ-valerolactone, 2-acetylbutyrolactone, triethylene glycol, diethylene glycol, ethylene glycol, ethylenediaminetetraacetic acid (EDTA), maleic acid, malonic acid, citric acid, acetic acid, oxalic acid, gluconic acid, glucose, fructose, sucrose, sorbitol, xylitol, γ-ketovaleric acid, di(C1-C4 alkyl) succinate, and more particularly dimethyl succinate, dimethylformamide, 1-methyl-2-pyrrolidone, propylene carbonate, 2-methoxyethyl 3-oxobutyrate, N,N-dihydroxyethylglycine, N-tris(hydroxymethyl)methylglycine, 2-furancarboxaldehyde (also known as furfural), 5-hydroxymethylfurfural (also known as 5-(hydroxymethyl)-2-furfuralcarboxaldehyde or 5-HMF), 2-acetylfuran, 5 -methyl-2-furaldehyde, ascorbic acid, butyl lactate, ethyl lactate, butyl butyrolactate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, 2-ethoxyethyl acetate, 2-butoxyethyl acetate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 1,5-pentanediol, 1-(2-hydroxyethyl)-2-pyrrolidinedione, 1-(-2-hydroxyethyl)-2,5-pyrrolidinedione, 5-methyl-2(3H)-furanone, 1-methyl-2-piperidone, 4-aminobutyric acid, butyl glycolate, ethyl 2-mercaptopropionate, ethyl 4-oxopentanoate, diethyl maleate, dimethyl maleate, dimethyl fumarate, diethyl fumarate, dimethyl adipate and dimethyl 3-oxoglutarate.

[0111] When it / they are present, the total content of (one or more) oxygen-containing organic compounds and / or nitrogen-containing organic compounds and / or sulfur-containing organic compounds present in the catalyst is generally 1 wt.% to 30 wt.%, preferably 1.5 wt.% to 25 wt.%, and more preferably 2 wt.% to 20 wt.%, relative to the total weight of the catalyst.

[0112] In catalyst preparation processes requiring a drying stage, the introduction of the organic compound is followed by a drying stage(s) at a temperature below 200° C., so as to preferably maintain at least 30%, preferably at least 50%, and very preferably at least 70% of the amount of organic compound introduced, calculated on the carbon remaining on the catalyst. The residual carbon is measured by elemental analysis according to ASTM D5373.

[0113] According to one embodiment, the catalyst according to the invention comprises and preferably consists of a support based on alumina or silica or silica-alumina, an active phase consisting of nickel, molybdenum and tungsten and phosphorus, characterized in that:

[0114] - a nickel content, measured in the form of NiO, of 3% to 4% by weight, preferably of 3.1% to 3.9% by weight and more preferably of 3.2% to 3.8% by weight, relative to the total weight of the catalyst,

[0115] - a molybdenum content, measured in the form of MoO3, of 2% to 4% by weight, preferably of 2.2% to 3.8% by weight and more preferably of 2.5% to 3.5% by weight, relative to the total weight of the catalyst,

[0116] - a tungsten content, measured in the form of WO3, of 34% to 40% by weight, preferably of 35% to 39.9% by weight and more preferably of 36% to 39% by weight, relative to the total weight of the catalyst,

[0117] - a phosphorus content, measured in the form of P2O5, of 3% to 4% by weight, preferably of 3.1% to 3.9% by weight and more preferably of 3.2% to 3.8% by weight, relative to the total weight of the catalyst,

[0118] - WO3 / MoO3 molar ratio is 5.3 to 12.4 mol / mol, preferably 5.7 to 11.1 mol / mol, and more preferably 6.4 to 9.7 mol / mol,

[0119] - NiO / (WO3+MoO3) molar ratio is 0.20 to 0.33 mol / mol, preferably 0.21 to 0.31 mol / mol, and more preferably 0.22 to 0.30 mol / mol,

[0120] The P2O5 / (WO3+MoO3) molar ratio is 0.21 to 0.34 mol / mol, preferably 0.22 to 0.33 mol / mol, and more preferably 0.23 to 0.32 mol / mol.

[0121] According to another embodiment, the catalyst according to the invention comprises and preferably consists of a support based on alumina or silica or silica-alumina, an active phase consisting of nickel, molybdenum and tungsten, and phosphorus, and oxygen-containing organic compounds and / or nitrogen-containing organic compounds and / or sulfur-containing organic compounds, characterized in that:

[0122] - a nickel content, measured in the form of NiO, of 3% to 4% by weight, preferably of 3.1% to 3.9% by weight and more preferably of 3.2% to 3.8% by weight, relative to the total weight of the catalyst,

[0123] - a molybdenum content, measured in the form of MoO3, of 2% to 4% by weight, preferably of 2.2% to 3.8% by weight and more preferably of 2.5% to 3.5% by weight, relative to the total weight of the catalyst,

[0124] - a tungsten content, measured in the form of WO3, of 34% to 40% by weight, preferably of 35% to 39.9% by weight and more preferably of 36% to 39% by weight, relative to the total weight of the catalyst,

[0125] - a phosphorus content, measured in the form of P2O5, of 3% to 4% by weight, preferably of 3.1% to 3.9% by weight and more preferably of 3.2% to 3.8% by weight, relative to the total weight of the catalyst,

[0126] - WO3 / MoO3 molar ratio is 5.3 to 12.4 mol / mol, preferably 5.7 to 11.1 mol / mol, and more preferably 6.4 to 9.7 mol / mol,

[0127] - NiO / (WO3+MoO3) molar ratio is 0.20 to 0.33 mol / mol, preferably 0.21 to 0.31 mol / mol, and more preferably 0.22 to 0.30 mol / mol,

[0128] The P2O5 / (WO3+MoO3) molar ratio is 0.21 to 0.34 mol / mol, preferably 0.22 to 0.33 mol / mol, and more preferably 0.23 to 0.32 mol / mol.

[0129] According to this embodiment, the organic compound is preferably selected from the group consisting of γ-valerolactone, 2-acetylbutyrolactone, triethylene glycol, diethylene glycol, ethylene glycol, ethylenediaminetetraacetic acid (EDTA), maleic acid, malonic acid, citric acid, acetic acid, gluconic acid, glucose, fructose, sucrose, sorbitol, xylitol, γ-ketovaleric acid, di(C1-C4-alkyl) succinates and more particularly dimethyl succinate, dimethylformamide, 1-methyl-2-pyrrolidone, propylene carbonate, 2-methoxyethyl 3-oxobutyrate, N,N-dihydroxyethylglycine, N-tris(hydroxymethyl)methylglycine, 2-furfural (also known as furfural), 5-hydroxymethylfurfural (also known as 5-(hydroxymethyl)-2-furfural or 5-HMF), 2-acetylfuran, 5-methyl- 2-Furaldehyde, ascorbic acid, butyl lactate, ethyl lactate, butyl butyrolactate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, 2-ethoxyethyl acetate, 2-butoxyethyl acetate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 1,5-pentanediol, 1-(2-hydroxyethyl)-2-pyrrolidinedione, 1-(-2-hydroxyethyl)-2,5-pyrrolidinedione, 5-methyl-2(3H)-furanone, 1-methyl-2-piperidone, 4-aminobutyric acid, butyl glycolate, ethyl 2-mercaptopropionate, ethyl 4-oxopentanoate, diethyl maleate, dimethyl maleate, dimethyl fumarate, diethyl fumarate, dimethyl adipate, and dimethyl 3-oxoglutarate.

[0130] Preparation method

[0131] The catalyst according to the present invention can be prepared according to any method for preparing supported catalysts known to those skilled in the art.

[0132] The catalyst according to the invention can be prepared according to a preparation method comprising the following stages:

[0133] a) contacting at least one nickel precursor, at least one molybdenum precursor and at least one tungsten precursor and phosphorus with a support based on alumina or silica or silica-alumina, so as to obtain a catalyst precursor

[0134] b) drying said catalyst precursor obtained from stage a) at a temperature below 200° C.,

[0135] c) optionally, calcining the catalyst precursor obtained in stage b) at a temperature of 200° C. to 550° C.,

[0136] d) Optionally, sulphurizing the catalyst obtained in stage b) or stage c).

[0137] The catalyst according to the invention can be prepared by impregnating the metallic nickel, molybdenum and tungsten and phosphorus onto the chosen support during the contacting operation of stage a). For example, the impregnation can be carried out according to the method known to those skilled in the art under the technical term dry impregnation, wherein only the required elemental amounts are introduced in the form of soluble salts into the chosen solvent, for example demineralized water, in order to fill the porosity of the support as completely as possible.

[0138] The precursors of the active phase based on nickel, molybdenum and tungsten and phosphorus can be introduced simultaneously or successively. The impregnation of each precursor can advantageously be carried out at least twice. Thus, it can be advantageous to impregnate the different precursors successively with different impregnation and aging times. One of the precursors can also be impregnated several times.

[0139] Preferably, an active phase based on nickel, molybdenum and tungsten and a precursor of phosphorus are introduced simultaneously.

[0140] The nickel precursor that can be used is advantageously selected from nickel oxide, nickel hydroxide, nickel hydroxycarbonate, nickel carbonate and nickel nitrate; preference is given to using, for example, nickel hydroxycarbonate, nickel carbonate or nickel hydroxide.

[0141] The molybdenum precursors that can be used are well known to those skilled in the art. For example, among the sources of molybdenum, oxides and hydroxides, molybdic acid and its salts, in particular ammonium salts, such as ammonium molybdate and ammonium heptamolybdate, phosphomolybdic acid (HPMo), 12 O 40 ) and its salts, and optionally silicomolybdic acid (H4SiMo 12 O 40 ) and salts thereof. The source of molybdenum may also be, for example, a Keggin-type, vacant Keggin-type, substituted Keggin-type, Dawson-type, Anderson-type or Strandberg-type heteropoly compound. Molybdenum trioxide and a Strandberg-type, Keggin-type, vacant Keggin-type or substituted Keggin-type heteropoly anion are preferably used.

[0142] The tungsten precursors that can be used are also well known to those skilled in the art. For example, among the sources of tungsten, oxides and hydroxides, tungstic acid and its salts, in particular ammonium salts, such as ammonium tungstate and ammonium metatungstate, phosphotungstic acid and its salts, and optionally silicotungstic acid (H4SiW 12 O 40 ) and their salts. The source of tungsten may also be, for example, a Keggin-type, a vacant Keggin-type, a substituted Keggin-type or a Dawson-type heteropoly compound. Preferably, oxides and ammonium salts, such as ammonium metatungstate, or Keggin-type, vacant Keggin-type or a substituted Keggin-type heteropoly anion are used.

[0143] The phosphorus may be introduced in whole or in part by impregnation. Preferably, the phosphorus is introduced by impregnation, preferably dry impregnation, using a solution containing a nickel precursor, a molybdenum precursor and a tungsten precursor.

[0144] The phosphorus can advantageously be introduced alone or as a mixture with nickel, molybdenum and / or tungsten, and this can be done during any impregnation stage of the hydrogenation functional precursors (if these are introduced in several portions). If the oxygen-containing organic compound and / or the nitrogen-containing organic compound and / or the sulfur-containing organic compound are introduced separately from the hydrogenation functional precursors (the case of post-impregnation and pre-impregnation described hereinafter), the phosphorus can also be introduced in whole or in part during the impregnation of the oxygen-containing organic compound and / or the nitrogen-containing organic compound and / or the sulfur-containing organic compound. The phosphorus can also be introduced at any stage of the support synthesis, starting from the synthesis of the support. Thus, the phosphorus can be introduced before, during or after kneading with the selected alumina gel matrix, for example and preferably the aluminum oxyhydroxide (boehmite) of the alumina precursor.

[0145] The preferred phosphorus precursor is orthophosphoric acid H3PO4, but its salts and esters, such as ammonium phosphate, are also suitable. Phosphorus can also be introduced simultaneously with the element(s) from Group VIb in the form of Keggin-type, occlusive Keggin-type, substituted Keggin-type or Strandberg-type heteropolyanions.

[0146] Any impregnation solution described in the present invention may contain any polar solvent known to those skilled in the art. The polar solvent used is advantageously selected from methanol, ethanol, water, phenol and cyclohexanol, used alone or as a mixture. Preferably, a polar aprotic solvent is used. A list of commonly used polar solvents and their dielectric constants can be found in the book "Solvents andSolvent Effects in Organic Chemistry" (C. Reichardt, Wiley-VCH, 3rd edition, 2003, pp. 472-474). Very preferably, the solvent used is water or ethanol, and particularly preferably, the solvent is water.

[0147] When the catalyst additionally comprises a dopant selected from boron, fluorine or a mixture of boron and fluorine, the dopant(s) may be introduced at various stages of the preparation and in various ways in the same manner as described above for the introduction of phosphorus.

[0148] The boron precursor may be boric acid, orthoboric acid H3BO3, ammonium diborate or ammonium pentaborate, boron oxide or a boric ester. Boron may be introduced, for example, by a solution of boric acid in a water / alcohol mixture or in a water / ethanolamine mixture. Preferably, if boron is introduced, the boron precursor is orthoboric acid.

[0149] Fluorine precursors that can be used are well known to those skilled in the art. For example, fluoride anions can be introduced in the form of hydrofluoric acid or its salts. These salts are formed in the form of alkali metals, ammonium salts or organic compounds. In the latter case, the salt is advantageously formed in the reaction mixture by the reaction between the organic compound and hydrofluoric acid. Fluorine can be introduced, for example, by impregnation of an aqueous solution of hydrofluoric acid, or ammonium fluoride, or ammonium difluoride.

[0150] When the catalyst additionally comprises oxygen-containing organic compounds and / or nitrogen-containing organic compounds and / or sulfur-containing organic compounds, the latter are introduced before the drying stage b). The organic compounds are usually introduced by impregnation in the presence or absence of nickel, molybdenum, tungsten and phosphorus and in the presence or absence of solvents.

[0151] The introduction of the organic compound comprises a variety of embodiments, which differ in particular in the timing of the introduction of the organic compound relative to the introduction of the metal. It can be carried out at the same time as the metal impregnation (co-impregnation), or after the metal impregnation (post-impregnation), or finally before the metal impregnation (pre-impregnation), in particular during the preparation of the support, and preferably during the shaping process or by impregnation on a preformed support. Each embodiment used alone or in combination can be carried out in one or more stages.

[0152] Furthermore, the contacting stage may combine at least two embodiments, such as co-impregnation and post-impregnation. According to an alternative embodiment, the contacting operation according to stage a) combines at least two contacting embodiments, such as co-impregnation of nickel, molybdenum, tungsten and phosphorus with an organic compound, followed by drying at a temperature below 200° C., followed by post-impregnation with an organic compound that may be the same or different from the organic compound used for co-impregnation. Each embodiment, used alone or in combination, may be carried out in one or more stages.

[0153] The organic compound(s) are advantageously introduced into the impregnation solution, which, according to the manufacturing embodiment, can be the same or different solution as the solution comprising the nickel precursor, the molybdenum precursor and the tungsten precursor and phosphorus, in an amount corresponding to:

[0154] the molar ratio of the organic compound to the sum of the elements of group VIb (Mo and W) of the catalyst precursor is from 0.01 to 5 mol / mol, preferably from 0.05 to 3 mol / mol, preferably from 0.05 to 1.5 mol / mol and very preferably from 0.1 to 1.2 mol / mol, calculated on the components introduced into the impregnation solution(s), and

[0155] The molar ratio of the organic compound to the group VIII element (Ni) of the catalyst precursor is from 0.02 to 17 mol / mol, preferably from 0.1 to 10 mol / mol, preferably from 0.15 to 8 mol / mol and very preferably from 0.6 to 5 mol / mol, calculated on the components introduced into the impregnation solution(s).

[0156] When several organic compounds are present, different molar ratios apply for each organic compound present.

[0157] Advantageously, after each impregnation stage, the impregnated support is ripened. Ripening allows the impregnation solution to diffuse and the precursor to be evenly dispersed within the support.

[0158] Any aging stage described in the present invention is advantageously carried out at atmospheric pressure, in a water-saturated atmosphere, and at a temperature of 17° C. to 50° C., and preferably at ambient temperature. Typically, an aging time of 10 minutes to 48 hours, and preferably 30 minutes to 5 hours, is sufficient. Longer time periods are not excluded, but do not necessarily lead to improvements.

[0159] According to stage b) of the preparation process according to the invention, the optionally aged catalyst precursor obtained in stage a) is subjected to a drying stage at a temperature below 200° C., preferably from 50° C. to 180° C., preferably from 70° C. to 150° C. and very preferably from 75° C. to 130° C.

[0160] The drying stage is advantageously carried out by any technique known to the person skilled in the art. It is advantageously carried out at atmospheric pressure or at reduced pressure, and preferably at atmospheric pressure. It is advantageously carried out in a transverse bed using hot air or any other hot gas. Preferably, when the drying is carried out in a fixed bed, the gas used is air or an inert gas, such as argon or nitrogen. Very preferably, the drying is carried out in the presence of nitrogen and / or air in a transverse bed. Preferably, the drying stage has a short duration of 5 minutes to 4 hours, preferably 30 minutes to 4 minutes, and very preferably 1 hour to 3 hours. When an organic compound is present, the drying is then carried out to preferably keep at least 30% of the organic compound introduced; preferably, this amount is greater than 50%, and even more preferably greater than 70%, calculated based on the residual carbon on the catalyst. At the end of the drying stage b), a dried catalyst is obtained.

[0161] Optionally, the drying stage b) may be followed by a calcination stage c).

[0162] According to this alternative form, at the end of the drying stage b), a calcination stage c) is carried out at a temperature ranging from 200° C. to 600° C., preferably from 250° C. to 550° C., in an inert atmosphere (for example nitrogen) or under an oxygen-containing atmosphere (for example air). The duration of this heat treatment is generally between 0.5 hours and 16 hours, preferably between 1 hour and 5 hours. After this treatment, the active phase is therefore generally found in the form of an oxide; the heteropolyanions are thus converted into oxides. Similarly, when the catalyst is introduced, it no longer contains organic compounds or contains very small amounts of organic compounds. However, the introduction of organic compounds during its preparation makes it possible to increase the dispersion of the active phase, thus producing a more active catalyst.

[0163] When organic compounds are present, the catalyst is preferably not calcined. Calcination is understood in this context to mean a heat treatment at a temperature greater than or equal to 200° C. under an air- or oxygen-containing gas.

[0164] However, it is possible to subject the catalyst precursor to a calcination stage before the introduction of the organic compounds, in particular after the impregnation of nickel, molybdenum and tungsten and phosphorus.

[0165] The catalyst according to the invention may be a fresh catalyst, ie a catalyst which has not been used previously as catalyst in a catalytic unit, and in particular in hydrotreatment and / or hydrocracking.

[0166] The catalyst according to the invention may also be a regenerated and / or reactivated catalyst. A regenerated and / or reactivated catalyst is understood to mean a catalyst which has been used as a catalyst in a catalytic unit, and in particular in a hydroprocessing and / or hydrocracking, and has undergone at least one stage of partial or complete removal of coke, for example by calcination (regeneration). Regeneration may be carried out by any means known to those skilled in the art. Regeneration is generally carried out by calcining at a temperature of 350°C to 550°C, and generally at a temperature of 400°C to 520°C, or 420°C to 520°C, or 450°C to 520°C, with temperatures below 500°C generally being advantageous.

[0167] When the regenerated catalyst no longer comprises enough active phase or phosphorus, or when it exhibits one or more ratios outside the described ratio, the regenerated catalyst can be reactivated by introducing one or more precursors of active phase and / or phosphorus into the regenerated catalyst. It is also possible to introduce at least one organic compound simultaneously or separately with metal and phosphorus. When the catalyst comprises such an organic compound, the organic compound introduced can be the same or different from the organic compound of the fresh catalyst. Of course, the above-mentioned operating conditions about slaking, drying and optional calcination and optional sulfidation are also applicable in the context of this last embodiment.

[0168] Before using it in hydrotreatment and / or hydrocracking reactions, it is advantageous to convert the catalyst obtained according to any of the modes of introduction described in the present invention into a sulphurized catalyst to form its active entity. This activation or sulphurization stage is carried out by methods well known to those skilled in the art and is advantageously carried out in the presence of hydrogen and hydrogen sulphide under a sulphur reducing atmosphere.

[0169] According to one alternative form, the catalyst is advantageously subjected to a sulphurization stage after the drying b) or the optional calcination stage c).

[0170] Advantageously, the catalyst is subjected to non-original or original situ sulfidation. The sulfiding agent is H2S gas, elemental sulfur, CS2, mercaptan, sulfide and / or polysulfide, a hydrocarbon fraction with a boiling point lower than 400°C, the hydrocarbon fraction containing sulphur compounds or any other sulphur-containing compounds used to activate hydrocarbon feedstock for the purpose of sulfiding catalyst. The sulphur-containing compounds are advantageously selected from alkyl disulfides such as dimethyl disulfide (DMDS), alkyl sulfides such as dimethyl sulfide, mercaptans such as n-butyl mercaptan (or 1-butyl mercaptan), and polysulphide compounds of tertiary nonyl polysulphide types. The catalyst can also be sulfided by the sulphur contained in the feedstock to be desulfurized. Preferably, the catalyst is sulfided in situ in the presence of a sulfiding agent and a hydrocarbon feedstock. Very preferably, the catalyst is sulfided in situ in the presence of a hydrocarbon feedstock using dimethyl disulfide as an additive.

[0171] Hydrotreating and / or hydrocracking processes

[0172] Finally, another subject of the present invention is the use of the catalyst according to the invention or of the catalyst prepared by the preparation process according to the invention in processes for the hydrotreatment and / or hydrocracking of hydrocarbon fractions.

[0173] The catalyst according to the invention, which has preferably previously been subjected to a sulphurization stage, is advantageously used in hydrotreatment and / or hydrocracking reactions of hydrocarbon feedstocks, such as petroleum fractions, fractions derived from coal or hydrocarbons derived from natural gas, optionally as a mixture, or also hydrocarbon fractions derived from biomass, and more particularly in hydrogenation, hydrodenitrogenation, hydrodearomatization, hydrodesulfurization, hydrodeoxygenation, hydrodemetallization or hydroconversion reactions of hydrocarbon feedstocks.

[0174] In these applications, the catalyst according to the invention, which has preferably been previously subjected to a sulphurization stage, has an improved activity compared to the catalysts of the prior art. The catalyst can also be advantageously used in the pretreatment of catalytic cracking or hydrocracking feedstocks, or in the hydrodesulfurization of residues or in the forced hydrodesulfurization of gas oils (ULSD: Ultra Low Sulfur Diesel).

[0175] The feedstocks used in the hydrotreatment processes are, for example, gasoline, gas oils, vacuum gas oils, atmospheric residues, vacuum residues, atmospheric distillates, vacuum distillates, heavy fuel oils, oils, waxes and paraffins, waste oils, deasphalted residues or crude oils, feedstocks originating from thermal or catalytic conversion processes, lignocellulosic feedstocks or, more generally, feedstocks originating from biomass, such as vegetable oils, used alone or as a mixture. The feedstocks treated, and in particular the above-mentioned feedstocks, generally contain heteroatoms, such as sulphur, oxygen and nitrogen, and in the case of heavy feedstocks, they generally also contain metals.

[0176] The operating conditions used in the process of implementing the above-mentioned hydrocarbon feedstock hydroprocessing reaction are generally as follows: the temperature is advantageously 180°C to 450°C, and preferably 250°C to 440°C, the pressure is advantageously 0.5 to 30 MPa, and preferably 1 to 18 MPa, and the hourly space velocity is advantageously 0.1 to 20 h -1 , and preferably 0.2 to 5h -1 , and the hydrogen / feedstock ratio, expressed as the volume of hydrogen per volume of liquid feedstock measured under standard temperature and pressure conditions, is advantageously between 50 l / l and 5000 l / l and preferably between 80 l / l and 2000 l / l.

[0177] According to a first mode of use, the hydrotreatment process according to the invention is a process of hydrotreatment of a gas-oil fraction, and in particular of hydrodesulfurization (HDS), carried out in the presence of at least one catalyst according to the invention. The hydrotreatment process according to the invention aims to remove sulfur-based compounds present in the gas-oil fraction in order to meet the current environmental standards, i.e., sulfur contents permitted of at most 10 ppm. It is also possible to reduce the content of aromatics and nitrogen in the gas-oil fraction to be hydrotreated.

[0178] According to the process of the invention, the gas oil fraction to be hydrotreated contains from 0.02% to 5.0% by weight of sulfur. It advantageously originates from straight run distillation (or straight run gas oil), a coking unit, a visbreaking unit, a steam cracking unit, a unit for hydrotreating and / or hydrocracking heavier feedstocks and / or a catalytic cracking unit (fluid catalytic cracking). The gas oil fraction preferably exhibits that at least 90% of its compounds have a boiling point of between 250° C. and 400° C. at atmospheric pressure.

[0179] The process for hydrotreating the gas oil fraction according to the present invention is carried out under the following operating conditions: a temperature of 200 to 400° C., preferably 300 to 380° C., a total pressure of 2 to 10 MPa, and more preferably 3 to 8 MPa, a ratio of the volume of hydrogen / the volume of the hydrocarbon feedstock expressed as the volume of hydrogen per volume of the liquid feedstock measured under standard temperature and pressure conditions of 100 to 600 liters / liter, and more preferably 200 to 400 liters / liter, and an hourly space velocity (HSV) of 0.5 to 10 h-1 , preferably 0.7 to 8h -1 .

[0180] HSV corresponds to the inverse of the contact time expressed in hours and is defined by the ratio of the volume flow rate of the liquid hydrocarbon feedstock / the volume of the catalyst loaded into the reaction unit implementing the hydrotreatment process according to the invention. The reaction unit implementing the process for hydrotreating the gas oil fraction according to the invention is preferably operated as a fixed bed, a moving bed, or an ebullating bed, preferably as a fixed bed.

[0181] According to a second mode of use, the hydrotreatment and / or hydrocracking process according to the invention is a process of hydrotreatment (in particular hydrodesulfurization, hydrodenitrogenation, hydrogenation of aromatics) and / or hydrocracking of a vacuum distillate fraction carried out in the presence of at least one catalyst according to the invention. The hydrotreatment and / or hydrocracking process, also known as hydrocracking or hydrocracking pretreatment process according to the invention, is intended to remove the sulfur-based compounds, nitrogen-based compounds or aromatic compounds present in the distillate fraction, as the case may be, in order to pretreat it before the conversion in a catalytic cracking or hydroconversion process, or to hydrocracking a distillate fraction that may optionally have been previously pretreated, if necessary.

[0182] A wide variety of feedstocks can be treated by the above-mentioned process of hydrotreating and / or hydrocracking the vacuum distillate. Typically, they contain at least 20% by volume, and typically at least 80% by volume, of compounds having a boiling point higher than 340°C at atmospheric pressure. The feedstock may be, for example, a vacuum distillate, or a feedstock produced from a unit for extracting aromatics from a lubricating oil base, or a feedstock produced from solvent dewaxing of a lubricating oil base, and / or a feedstock produced from deasphalted oil, or the feedstock may be deasphalted oil or paraffin produced from a Fischer-Tropsch process, or any mixture of the feedstocks mentioned above. Typically, the feedstock has a T5 boiling point higher than 340°C at atmospheric pressure, and more preferably has a T5 boiling point higher than 370°C at atmospheric pressure, i.e. 95% of the compounds present in the feedstock have a boiling point higher than 340°C, and more preferably higher than 370°C. The nitrogen content of the feedstock treated in the process according to the invention is typically greater than 200 ppm by weight, preferably from 500 to 10,000 ppm by weight. The sulfur content of the feedstock treated in the process according to the invention is typically between 0.01% and 5.0% by weight. The feedstock may optionally contain metals such as nickel and vanadium. The asphaltene content is typically less than 3000 ppm by weight.

[0183] Usually at a temperature higher than 200°C, usually 250°C to 480°C, advantageously 320°C to 450°C, preferably 330°C to 435°C, at a pressure higher than 1 MPa, usually 2 to 25 MPa, preferably 3 to 20 MPa, for 0.1 to 20.0 h -1 , and preferably 0.1 to 6.0h -1 , preferably 0.2 to 3.0h -1 The hydrotreating and / or hydrocracking catalyst is contacted with the above feedstock in the presence of hydrogen at a space velocity of 1.5 % and the amount of hydrogen introduced is such that the volume ratio of liters of hydrogen / liters of hydrocarbon, expressed as the volume of hydrogen per volume of liquid feedstock measured under standard temperature and pressure conditions, is advantageously between 80 l / l and 5000 l / l, and generally between 100 l / l and 2000 l / l. These operating conditions used in the process according to the invention generally make it possible to obtain a single-pass conversion rate of greater than 15%, and more preferably between 20% and 95%, into a product having a boiling point of less than 340° C. at atmospheric pressure, and more preferably less than 370° C. at atmospheric pressure.

[0184] The process of hydrotreating and / or hydrocracking the vacuum distillate using the catalyst according to the invention covers a range of pressures and conversions from mild hydrocracking to high pressure hydrocracking. Mild hydrocracking is understood to mean hydrocracking which produces a moderate conversion of typically less than 40% and operates at a low pressure of typically 2 MPa to 6 MPa.

[0185] The catalyst according to the invention can be used alone, in one or more fixed catalytic beds, in one or more reactors, in a "one-step" hydrocracking scheme (with or without liquid recycle of the unconverted fraction), or in a "two-step" hydrocracking scheme, optionally in combination with a hydrorefining catalyst located upstream of the catalyst of the invention.

[0186] According to the third mode of use, the hydrotreating and / or hydrocracking process according to the present invention is advantageously carried out as pretreatment in a fluidized catalytic cracking (or FCC: fluid catalytic cracking) process. In terms of the range of temperature, pressure, hydrogen circulation rate and hourly space velocity, the operating conditions of the pretreatment are generally the same as the operating conditions described above for the hydrotreating and / or hydrocracking process of the vacuum distillate. The FCC process can be carried out under suitable cracking conditions in a conventional manner known to those skilled in the art to produce hydrocarbon products with lower molecular weight. A brief description of catalytic cracking can be found in, for example, Ullmann's Encyclopedia of Industrial Chemistry, Vol. A18, 1991, pp. 61-64.

[0187] According to a fourth mode of use, the hydrotreatment and / or hydrocracking process according to the invention is a process for hydrotreating (in particular hydrodesulfurizing) a gasoline fraction in the presence of at least one catalyst according to the invention.

[0188] Unlike other hydrotreating processes, gasoline hydrotreating (particularly hydrodesulfurization) must be able to resolve dual conflicting constraints: providing deep hydrodesulfurization of gasoline and limiting the hydrogenation of unsaturated compounds present to limit octane loss.

[0189] The feedstock is generally a hydrocarbon fraction having a distillation range from 30 to 260° C. Preferably, the hydrocarbon fraction is a gasoline-type fraction. Very preferably, the gasoline fraction is an olefinic gasoline fraction resulting, for example, from a catalytic cracking (fluid catalytic cracking) unit.

[0190] The hydrotreating process comprises contacting the hydrocarbon fraction with a catalyst according to the present invention and hydrogen under the following conditions: at a temperature of 200 to 400° C., preferably 230 to 330° C., at a total pressure of 1 to 3 MPa, preferably 1.5 to 2.5 MPa, for 1 to 10 h. -1 , preferably 2 to 6 hours -1 The hourly space velocity (HSV) is defined as the volume flow rate of the feed relative to the volume of the catalyst, and at a volume ratio of hydrogen / gasoline feed of 100 to 600 Sl / l, preferably 200 to 400 Sl / l.

[0191] The process of hydrotreating gasoline can be carried out in one or more reactors of the fixed bed type or the ebullating bed type connected in series. If the process is carried out with the aid of at least two reactors connected in series, a device can be provided for removing H2S from the effluent produced in the first hydrodesulfurization reactor before treating the effluent in the second hydrodesulfurization reactor. Example

[0192] The following examples show that the activity of the catalyst according to the invention is significantly improved compared to the catalysts of the prior art.

[0193] Examples 1 to 10 describe the preparation of catalysts C1 to C10. The final composition of each catalyst in terms of metals and phosphorus, expressed in the form of oxides and relative to the weight of the catalyst, as well as the WO3 / MoO3, NiO / (WO3+MoO3) and P2O5 / (WO3+MoO3) ratios are shown in Table 1 below.

[0194] Examples 1 to 6 describe the preparation of catalysts C1 to C6 not in accordance with the invention, whose WO3 / MoO3, NiO / (WO3+MoO3) or P2O5 / (WO3+MoO3) ratios are respectively lower and higher than the claimed range.

[0195] Examples 7 to 10 describe the preparation of catalysts C7 to C10 according to the present invention, whose WO3 / MoO3, NiO / (WO3+MoO3) or P2O5 / (WO3+MoO3) ratios are respectively within the claimed range.

[0196] Example 1: Preparation of the catalyst NiMoWP C1 on alumina (not in accordance with the invention).

[0197] Nickel, molybdenum, tungsten and phosphorus were added to 100 g of alumina support A1, showing a loss on ignition of 4.9 wt%, a loss of 230 m 2 / g BET specific surface area, 0.78ml / g pore volume measured by mercury intrusion method and 11.5nm average pore diameter (defined as volume median diameter by mercury intrusion method), and provided in the form of "extrudate". The impregnation solution was prepared by dissolving molybdenum oxide (16.5g), ammonium metatungstate (55.9g), nickel nitrate (25.8g) and 10.2g of 85% by weight orthophosphoric acid solution in 78ml distilled water at 90°C. After dry impregnation, the extrudate was aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90°C for 16 hours. The dried catalyst thus obtained is recorded as C1.

[0198] Example 2: Preparation of the catalyst NiMoWP C2 on alumina (not in accordance with the invention).

[0199] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (1.9 g), ammonium metatungstate (82.5 g), nickel nitrate (25.8 g) and 10.2 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C2.

[0200] Example 3: Preparation of the catalyst NiMoWP C3 (not in accordance with the invention) on alumina.

[0201] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (6.1 g), ammonium metatungstate (74.8 g), nickel nitrate (18.2 g) and 10.2 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C3.

[0202] Example 4: Preparation of the catalyst NiMoWP C4 on alumina (not in accordance with the invention).

[0203] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (6.1 g), ammonium metatungstate (74.8 g), nickel nitrate (35.4 g) and 10.2 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C4.

[0204] Example 5: Preparation of the catalyst NiMoWP C5 on alumina (not in accordance with the invention).

[0205] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (6.1 g), ammonium metatungstate (74.8 g), nickel nitrate (25.8 g) and 7.2 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C5.

[0206] Example 6: Preparation of the catalyst NiMoWP C6 on alumina (not in accordance with the invention).

[0207] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (6.1 g), ammonium metatungstate (74.8 g), nickel nitrate (25.8 g) and 14.0 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C6.

[0208] Example 7: Preparation of the catalyst NiMoWP C7 (according to the invention) on alumina.

[0209] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (6.1 g), ammonium metatungstate (74.8 g), nickel nitrate (25.8 g) and 10.2 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C7.

[0210] Example 8: Preparation of the catalyst NiMoWP C8 (according to the invention) on alumina by co-impregnation of an organic compound (oxalic acid).

[0211] Nickel, molybdenum, tungsten and phosphorus were added to the alumina support in Example 1 above, and the support was provided in the form of "extrudates". The impregnation solution was prepared by dissolving molybdenum oxide (4.3 g), ammonium metatungstate (70.5 g), nickel nitrate (21.8 g) and 9.3 g of 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90°C. After homogenizing the aforementioned mixture, 6.7 g of oxalic acid was added before the volume of the solution was adjusted to the pore volume of the support by adding water. The (oxalic acid) / (Mo+W) molar ratio was equal to 0.25 mol / mol, and the (oxalic acid) / Ni molar ratio was equal to 1 mol / mol. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 120°C for 16 hours. The dried catalyst thus obtained and added with oxalic acid was recorded as C8.

[0212] Example 9 Preparation of the catalyst NiMoWP C9 (according to the invention) on alumina by post-addition of an organic compound (ascorbic acid).

[0213] 100 g of the catalyst C7 precursor described above in Example 3 and provided in the form of "extrudates" were impregnated with an aqueous solution containing 28.8 g of ascorbic acid and a volume equal to the pore volume of the catalyst C7 precursor. The amounts involved were such that the amount of ascorbic acid was 0.5 mol / mole of molybdenum and 0.5 mol / mole of tungsten (equivalent to 1.9 mol / mole of nickel). The extrudates were aged for 16 hours in a water-saturated atmosphere at ambient temperature. The catalyst C9 precursor was then dried at 120° C. for 2 hours to obtain catalyst C9.

[0214] Example 10 Preparation of the catalyst NiMoWP C10 (according to the invention) on silica-alumina by post-addition of an organic compound (1-methyl-2-pyrrolidone).

[0215] Nickel, molybdenum, tungsten and phosphorus were added to a silica-alumina support containing 10 wt% silicon and exhibited a loss on ignition of 0.7 wt%, a 2 / g BET specific surface area, 0.45ml / g pore volume measured by mercury intrusion method and 7.3nm average pore diameter (defined as volume median diameter by mercury intrusion method), and provided in the form of "extrudates". The impregnation solution was prepared by dissolving molybdenum oxide (4.6g), ammonium metatungstate (75.8g), nickel nitrate (25.3g) and 11.1g of 85% by weight orthophosphoric acid solution in 55.7ml distilled water at 90°C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90°C for 16 hours. The catalyst precursor was then impregnated with an aqueous solution containing 25.9g of 1-methyl-2-pyrrolidone and a volume equal to the pore volume of the catalyst C7 precursor. The amounts involved were such that the amount of 1-methyl-2-pyrrolidone was 0.8mol / mole of molybdenum and 0.8mol / mole of tungsten (equivalent to 3.0mol / mole of nickel). The extrudates were aged in a water-saturated atmosphere at ambient temperature for 16 hours. The catalyst C10 precursor was then dried at 120° C. for 2 hours to obtain catalyst C10.

[0216] Example 11: Preparation of the catalyst NiMoWP C11 on alumina (comparative).

[0217] Nickel, molybdenum, tungsten and phosphorus were added to the same support A1 as shown in Example 1. The impregnation solution was prepared by dissolving molybdenum oxide (7.7 g), ammonium metatungstate (85.3 g), nickel nitrate (37.6 g) and 7.5 g of an 85 wt% orthophosphoric acid solution in 78 ml of distilled water at 90° C. After dry impregnation, the extrudates were aged in a water-saturated atmosphere at ambient temperature for 24 hours and then dried at 90° C. for 16 hours. The dried catalyst thus obtained was designated C11.

[0218] Example 12: Preparation of the catalyst NiMoWP C12 (comparative) on alumina by post-addition of an organic compound (citric acid).

[0219] 100 g of the catalyst C11 precursor provided in the form of "extrudates" were impregnated with an aqueous solution containing 7.8 g of citric acid and a volume equal to the pore volume of the catalyst C11 precursor. The amounts involved were such that the (citric acid) / (NiO+MoO3+WO3) molar ratio was 0.08. The extrudates were aged for 16 hours in a water-saturated atmosphere at ambient temperature. The catalyst C12 precursor was then dried at 120° C. for 2 hours to obtain catalyst C12.

[0220] Example 13 Preparation of the catalyst NiMoWP C13 (according to the invention) on alumina by post-addition of an organic compound (citric acid).

[0221] 100 g of the catalyst C7 precursor of the present patent application and provided in the form of "extrudates" were impregnated with an aqueous solution containing 6.4 g of citric acid and a volume equal to the pore volume of the catalyst C7 precursor. The amounts involved were such that the (citric acid) / (NiO+MoO3+WO3) molar ratio was 0.08. The extrudates were aged for 16 hours in a water-saturated atmosphere at ambient temperature. The catalyst C13 precursor was then dried at 120°C for 2 hours to obtain catalyst C13.

[0222] Example 14: Catalyst C1, Catalyst C2, Catalyst C3, Catalyst C4, Catalyst C5, Catalyst C6, Catalyst C11 and Catalyst C12 (not in accordance with the invention) and Catalyst C7, Catalyst C8, Catalyst C9, Catalyst C10 and Catalyst C13 (in accordance with the invention) were evaluated in the hydrogenation of aromatics of gas oil (HDA).

[0223] Catalysts C1, C2, C3, C4, C5, C6, C11 and C12 (not in accordance with the invention) and C7, C8, C9, C10 and C13 (in accordance with the invention) were tested in the hydrogenation of aromatics of gas oil (HDA).

[0224] The feedstock is a mixture of 30% by volume of gas oil produced from atmospheric distillation (also called straight run distillation) and 70% by volume of light gas oil produced from a catalytic cracking unit (also called LCO, light cycle oil). The properties of the test feedstock used are as follows: Density at 15°C = 0.8994 g / cm 3 (NF EN ISO 12185), refractive index at 20° C. = 1.5143 (ASTM D1218-12), sulfur content = 0.38 wt. %, nitrogen content = 0.05 wt. %.

[0225] Simulated distillation (ASTM D2887):

[0226] -IP: 133℃

[0227] -10%: 223℃

[0228] -50%: 285℃

[0229] -90%: 357℃

[0230] -FP: 419℃

[0231] The tests were carried out in an isothermal pilot reactor with a transversely fixed bed, with the fluid circulating from the bottom upwards.

[0232] The gas oil feedstock (density at 15°C = 0.8491 g / cm2) was distilled at 350°C in a reactor under a certain pressure by atmospheric (straight run) distillation. 3 (NF EN ISO 12185), and initial sulfur content = 0.42 wt. %), the catalyst was previously sulfurized in situ, with the addition of 2 wt. % dimethyl disulfide.

[0233] The hydrogenation test of aromatics was carried out under the following operating conditions: total pressure of 8 MPa, catalyst volume of 4 cm 3 , temperature was 330°C, hydrogen flow rate was 3.0 l / h, and feed flow rate was 4.5 cm 3 / h.

[0234] The characteristics of the effluent were analyzed: density at 15°C (NF EN ISO 12185), refractive index at 20°C (ASTM D1218-12), simulated distillation (ASTM D2887), sulfur content and nitrogen content. The residual content of aromatic carbon was calculated by the ndM method (ASTM D3238). The degree of hydrogenation of aromatics was calculated by the ratio of the aromatic carbon content of the effluent to the aromatic carbon content of the test feed. The catalytic performance qualities of the tested catalysts are given in Table 1. They are expressed as relative volume activity (RVA) relative to the catalyst C7 chosen as reference, assuming an order of magnitude of 1.7 for the relevant reaction.

[0235] Table 1 clearly shows the gain in catalytic effect contributed by the specific formulation according to the invention. This is because catalysts C1, C2, C3, C4, C5, C6, C11 and C12 (not in accordance with the invention) show lower activities than the activity obtained with catalyst C7 (in accordance with the invention). Catalysts C8, C9, C10 and C13 (in accordance with the invention) also show higher activities than catalyst C7.

[0236] Table 1 clearly shows the gain in catalytic effect contributed by the specific formulation according to the invention. This is because the catalyst C11 (comparative) without additions shows a lower activity than the activity obtained with the catalyst C7 (according to the invention) without additions. Similarly, the catalyst C12 (comparative) with additions shows a lower activity than the activity obtained with the catalyst C13 (according to the invention) with additions. For both comparisons, only the contents and ratios of metals and phosphorus were modified.

[0237] The advantages of the catalyst according to the invention are therefore significant, regardless of the way in which it is prepared, and therefore have a higher efficiency than other compounds of the prior art.

[0238] Table 1 : Relative isovolumetric activities of catalysts C1, C2, C3, C4, C5 and C6 as well as catalysts C11 and C12 (not in accordance with the invention) and catalysts C8, C9, C10 and C13 (in accordance with the invention) in the hydrogenation of aromatics of gas oils compared to catalyst C7 (in accordance with the invention).

[0239]

[0240]

Claims

1. A catalyst comprising a support based on alumina or silica or silica-alumina and an active phase consisting of nickel, molybdenum and tungsten and phosphorus, characterized in that: - a nickel content of 3% to 4% by weight, measured in the form of NiO, relative to the total weight of the catalyst, - a molybdenum content of 2% to 4% by weight, measured in the form of MoO3, relative to the total weight of the catalyst, - a tungsten content, measured in the form of WO3, of 34% to 40% by weight, relative to the total weight of the catalyst, - a phosphorus content of 3% to 4% by weight, measured in the form of P2O5, relative to the total weight of the catalyst, -WO3 / MoO3 molar ratio is 5.3 to 12.4 mol / mol, -NiO / (WO3+MoO3) molar ratio is 0.20 to 0.33 mol / mol, -P2O5 / (WO3+MoO3) molar ratio is 0.21 to 0.34 mol / mol.

2. The catalyst according to claim 1, characterized in that: - a nickel content of 3.1% to 3.9% by weight, measured in the form of NiO, relative to the total weight of the catalyst, - a molybdenum content, measured in the form of MoO3, of 2.2% to 3.8% by weight, relative to the total weight of the catalyst, - a tungsten content, measured in the form of WO3, of 35% to 39.9% by weight relative to the total weight of the catalyst, - a phosphorus content of 3.1% to 3.9% by weight, measured in the form of P2O5, relative to the total weight of the catalyst, -WO3 / MoO3 molar ratio is 5.7 to 11.1 mol / mol, -NiO / (WO3+MoO3) molar ratio is 0.21 to 0.31 mol / mol, -P2O5 / (WO3+MoO3) molar ratio is 0.22 to 0.33 mol / mol.

3. The catalyst according to claim 2, characterized in that: - a nickel content of 3.2% to 3.8% by weight, measured in the form of NiO, relative to the total weight of the catalyst, - a molybdenum content, measured in the form of MoO3, of 2.5% to 3.5% by weight, relative to the total weight of the catalyst, - a tungsten content, measured in the form of WO3, of 36% to 39% by weight relative to the total weight of the catalyst, - a phosphorus content of 3.2% to 3.8% by weight, measured in the form of P2O5, relative to the total weight of the catalyst, -WO3 / MoO3 molar ratio is 6.4 to 9.7 mol / mol, -NiO / (WO3+MoO3) molar ratio is 0.22 to 0.30 mol / mol, -P2O5 / (WO3+MoO3) molar ratio is 0.23 to 0.32 mol / mol.

4. The catalyst according to any one of claims 1 to 3, wherein the density of the metal from group VIB, expressed as the number of atoms of said metal per unit area of ​​the catalyst, is from 5 to 12 metal atoms from group VIB / nm 2 catalyst. 5 . The catalyst according to claim 1 , further comprising an organic compound containing oxygen and / or nitrogen and / or sulfur.

6. The catalyst according to claim 5, wherein the organic compound is selected from compounds comprising one or more chemical functional groups or compounds comprising a furan ring, wherein the chemical functional groups are selected from carboxyl, alcohol, thiol, thioether, sulfone, sulfoxide, ether, aldehyde, ketone, ester, carbonate, amine, nitrile, imide, oxime, urea or amide functional groups.

7. The catalyst according to claim 5, wherein the organic compound is selected from sugars.

8. The catalyst according to claim 5, wherein the organic compound is selected from the group consisting of γ-valerolactone, 2-acetylbutyrolactone, triethylene glycol, diethylene glycol, ethylene glycol, ethylenediaminetetraacetic acid (EDTA), maleic acid, malonic acid, citric acid, acetic acid, oxalic acid, gluconic acid, glucose, fructose, sucrose, sorbitol, xylitol, γ-ketovaleric acid, dialkyl succinates wherein the alkyl group is a C1-C4 alkyl group, dimethylformamide, 1-methyl-2-pyrrolidone, propylene carbonate, 2-methoxyethyl 3-oxobutyrate, N,N-dihydroxyethylglycine, N-tris(hydroxymethyl)methylglycine, 2-furancarboxaldehyde (furfural), 5-hydroxymethylfurfural, 2-acetylfuran, 5-methyl-2-furfural, ascorbic acid acid, butyl lactate, ethyl lactate, butyl butyrolactate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, 2-ethoxyethyl acetate, 2-butoxyethyl acetate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 1,5-pentanediol, 1-(2-hydroxyethyl)-2-pyrrolidone, 1-(2-hydroxyethyl)-2,5-pyrrolidinedione, 5-methyl-2(3H)-furanone, 1-methyl-2-piperidone, 4-aminobutyric acid, butyl glycolate, ethyl 2-mercaptopropionate, ethyl 4-oxopentanoate, diethyl maleate, dimethyl maleate, dimethyl fumarate, diethyl fumarate, dimethyl adipate and dimethyl 3-oxoglutarate.

9. The catalyst according to claim 8, wherein the dialkyl succinate is dimethyl succinate. 10 . The catalyst according to claim 5 , wherein the content of the organic compound is 1 wt % to 30 wt % relative to the total weight of the catalyst.

11. The catalyst according to any one of claims 1 to 3, which is at least partially sulphided.

12. A method for preparing a catalyst according to any one of claims 1 to 11, comprising the following stages: a) contacting at least one nickel precursor, at least one molybdenum precursor and at least one tungsten precursor and phosphorus with a support based on alumina or silica or silica-alumina to obtain a catalyst precursor, b) drying the catalyst precursor resulting from stage a) at a temperature below 200°C.

13. Process for the preparation of a catalyst according to claim 12, additionally comprising a stage c) in which the catalyst obtained in stage b) is calcined at a temperature of 200°C to 550°C.

14. Process for the preparation of a catalyst according to any one of claims 12 and 13, which additionally comprises a stage d) in which the catalyst obtained in stage b) or stage c) is subjected to a sulphurization treatment.

15. Use of the catalyst according to any one of claims 1 to 11 in a process for the hydrotreatment and / or hydrocracking of hydrocarbon fractions.