Etchant and grain boundary etching method of rare earth tantalate ceramics
By using oxide molten salt and Yb2Si2O7 sol as etchants, grain boundary etching of rare earth tantalate ceramics at high temperatures solves the problem that the existing technology cannot clearly observe the morphology and size of ceramic grains, and achieves safety and efficiency. Observation of microstructure.
Patent Information
- Application Number
- CN202211665939.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The existing grain boundary etching methods for ceramic materials cannot effectively etch the grain boundaries of the entire sample, and the grain morphology and size cannot be clearly observed, and the acid and alkali chemical reagents used are hazardous.
An etchant is used, which contains oxide molten salt and corrosion promoter Yb2Si2O7, and reacts with the rare earth tantalate ceramic block at high temperature to perform grain boundary etching, avoiding the use of hazardous chemicals.
It achieves clear grain boundary etching of rare earth tantalate ceramics and can observe the grain morphology and size. It does not involve hazardous chemicals such as acids and alkalis, and has strong applicability.
Smart Images

Figure CN116004234B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic etching, and in particular relates to an etchant and a grain boundary etching method for rare earth tantalate ceramics. Background Art
[0002] Rare earth tantalate ceramics are expected to replace YSZ (Y2O3 stabilized ZrO2) as a new generation of thermal barrier coating materials for aircraft engines due to their low thermal conductivity, excellent high temperature performance and ferroelastic toughening characteristics. In order to clarify the relationship between the microstructure and performance of rare earth tantalate ceramics, it is necessary to observe the grain morphology and size inside the rare earth tantalate ceramics; in order to clarify the ferroelastic toughening mechanism of rare earth tantalates, it is also necessary to characterize the ferroelastic domain structure inside the grains. Therefore, it is of great significance to study the grain morphology and size inside rare earth tantalate ceramics.
[0003] There are few existing methods for grain boundary corrosion of ceramic materials. The commonly used methods are high-temperature thermal corrosion and acid-base chemical etching. The corrosion range is limited to the grain boundaries on the surface of the ceramic block. The grain boundaries of the entire sample cannot be etched, and the grain morphology and size of the entire sample cannot be clearly observed. In addition, chemical reagents such as acids and alkalis have certain hazards.
[0004] Therefore, there is an urgent need to provide a method for grain boundary etching of rare earth tantalate ceramics, which can perform grain boundary etching on rare earth tantalate ceramics and observe clear grain boundaries, grain morphology and size. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an etchant and a method for etching grain boundaries of rare earth tantalate ceramics. The etchant and etching method provided by the present invention can be used to etch grain boundaries of rare earth tantalate ceramics, and clear grain boundaries, grain morphology and size of the rare earth tantalate ceramics can be observed.
[0006] A first aspect of the present invention provides an etchant.
[0007] Specifically, an etchant comprises an oxide molten salt and an etching aid, wherein the composition of the oxide molten salt is a CaO-b MgO-c AlO 1.5 -d SiO2, wherein a=20-40, b=5-20, c=5-25, d=30-60, and a+b+c+d=100; the etching aid comprises Yb2Si2O7.
[0008] It should be noted that, in the etchant, the oxide molten salt and the etching aid are packaged and placed separately.
[0009] Preferably, the composition of the oxide molten salt is a CaO-b MgO-c AlO 1.5-d SiO2, wherein a=25-40, b=5-15, c=10-25, d=35-55, and a+b+c+d=100; further preferably, the composition of the oxide molten salt is a CaO-b MgO-c AlO 1.5 -d SiO2, wherein a=28-38, b=5-15, c=10-20, d=35-50, and a+b+c+d=100.
[0010] Preferably, the etching aid is Yb2Si2O7 sol.
[0011] Preferably, the preparation method of the oxide molten salt is as follows: weigh CaO, MgO, Al2O3 and SiO2 powders, ball mill, dry and sinter to obtain the oxide molten salt.
[0012] Preferably, the ball milling process is performed by wet ball milling for 12 to 24 hours at a rotation speed of 200 to 400 r / min using anhydrous ethanol as a medium.
[0013] Preferably, the sintering process is sintering at 1200-1400° C. for 12-48 hours.
[0014] Further preferably, the preparation method of the oxide molten salt is as follows: weigh CaO, MgO, Al2O3 and SiO2 powders according to the composition of the oxide molten salt, use anhydrous ethanol as the medium, and wet ball mill for 12 to 24 hours at a rotation speed of 200-400r / min; then dry in an oven at 60 to 80°C for 12 to 24 hours, and then pass through a 40-80 mesh sieve; sinter the sieved mixed powder at 1200 to 1400°C for 12 to 48 hours to obtain a molten salt; ball mill the molten salt again, dry it, and sieve it to obtain an oxide molten salt.
[0015] Preferably, the preparation method of the Yb2Si2O7 sol is as follows: Yb(NO3)3·5H2O and tetraethyl orthosilicate (TEOS) are dissolved in anhydrous ethanol and stirred to obtain Yb2Si2O7 sol.
[0016] Preferably, the molar ratio of Yb(NO3)3·5H2O to tetraethyl orthosilicate is 1:1.1 to 1:1.5.
[0017] Preferably, the molar ratio of Yb(NO3)3·5H2O to anhydrous ethanol is 1:6 to 1:12; further preferably, the molar ratio of Yb(NO3)3·5H2O to anhydrous ethanol is 1:8 to 1:12.
[0018] The second aspect of the present invention provides the use of the above-mentioned etchant.
[0019] Specifically, the above-mentioned etchant is applied to the grain boundary etching of rare earth tantalate ceramics.
[0020] Preferably, the rare earth tantalate includes one of yttrium tantalate, samarium tantalate, europium tantalate, gadolinium tantalate, dysprosium tantalate, holmium tantalate and erbium tantalate.
[0021] A third aspect of the present invention provides a method for etching grain boundaries of rare earth tantalate ceramics.
[0022] Specifically, a method for etching the grain boundaries of rare earth tantalate ceramics is provided, using the above-mentioned etchant for treatment, and comprises the following steps:
[0023] (1) soaking rare earth tantalate powder in an etching aid, centrifuging, and removing the upper layer of liquid to obtain wet rare earth tantalate powder;
[0024] (2) drying the wetted rare earth tantalate powder obtained in step (1), cold pressing the powder into a shape; and then performing a first cold isostatic pressing to obtain a preform;
[0025] (3) drying the preformed body prepared in step (2); and then performing a second cold isostatic pressing to obtain a green body;
[0026] (4) Sintering the green body prepared in step (3) to obtain a rare earth tantalate ceramic block; mixing an oxide molten salt with anhydrous ethanol, coating the mixture on the rare earth tantalate ceramic block, and then performing grain boundary etching.
[0027] Preferably, in step (1), the volume ratio of the rare earth tantalate powder to the etching aid is 1:2 to 1:5; further preferably, in step (1), the volume ratio of the rare earth tantalate powder to the etching aid is 1:3 to 1:5.
[0028] Preferably, in step (2), the cold press forming process is carried out at 5 to 10 MPa, and the holding time is 1 to 5 minutes.
[0029] Preferably, in step (2), the first cold isostatic pressing process is performed at a pressure of 200 to 300 MPa for 10 to 20 minutes; further preferably, in step (2), the first cold isostatic pressing process is performed at a pressure of 200 to 250 MPa for 10 to 15 minutes.
[0030] Preferably, in step (3), the drying process is to first dry the preform at 75-85°C for 18-36 hours, and then dry it at 110-130°C for 12-24 hours.
[0031] Preferably, in step (3), the second cold isostatic pressing process is performed at a pressure of 200 to 300 MPa for 10 to 20 minutes; further preferably, in step (3), the second cold isostatic pressing process is performed at a pressure of 200 to 250 MPa for 10 to 15 minutes.
[0032] In steps (2)-(3), after the rare earth tantalate powder is cold-pressed into shape, it is first cold isostatically pressed, then dried, and then cold isostatically pressed for a second time, which can effectively eliminate the pores in the green body and make the green body sample denser, which is conducive to the observation of clear grain boundaries after subsequent grain boundary etching. Because the Yb2Si2O7 sol will shrink after drying, resulting in a large number of pores in the block, the pores can be eliminated by secondary cold isostatic pressing, making the sample denser. Preferably, in step (4), the sintering process is to sinter the green body prepared in step (3) at 1550-1650°C for 12-48h.
[0033] Preferably, in step (4), the volume ratio of the oxide molten salt to anhydrous ethanol is 3:1 to 1:2; further preferably, in step (4), the volume ratio of the oxide molten salt to anhydrous ethanol is 2:1 to 1:2.
[0034] Preferably, in the coating process of step (4), the coating amount is 20 to 40 mg / cm 2 .
[0035] Preferably, in step (4), the grain boundary etching process is carried out at a temperature of 1250-1500° C. for 5-100 h; further preferably, in step (4), the grain boundary etching process is carried out at a temperature of 1300-1400° C. for 20-60 h.
[0036] More specifically, a method for etching grain boundaries of rare earth tantalate ceramics comprises the following steps:
[0037] (1) Soaking rare earth tantalate powder in Yb2Si2O7 sol at a volume ratio of 1:2 to 1:5, and shaking vigorously to make the rare earth tantalate powder fully wetted by the sol; then centrifuging to remove the upper layer of Yb2Si2O7 sol to obtain wetted rare earth tantalate powder;
[0038] (2) drying the wetted rare earth tantalate powder and cold pressing it at 5 to 10 MPa; then maintaining the pressure at 200 to 300 MPa for 10 to 20 minutes to complete the first cold isostatic pressing to obtain a preform;
[0039] (3) drying the preformed body prepared in step (2) at 75-85° C. for 18-36 h, and then drying at 110-130° C. for 12-24 h; after drying, maintaining the pressure at 200-300 MPa for 10-20 min, completing a second cold isostatic pressing, and obtaining a body;
[0040] (4) Sintering the green body prepared in step (3) at 1550-1650° C. for 12-48 h to obtain a rare earth tantalate ceramic block; mixing the oxide molten salt and anhydrous ethanol in a volume ratio of 3:1-1:2 and uniformly coating the mixture on the rare earth tantalate ceramic block, and then maintaining the mixture at 1250-1500° C. for 5-100 h to perform grain boundary etching.
[0041] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0042] (1) The present invention uses oxide molten salt and an etching aid (preferably Yb2Si2O7 sol) as an etchant to etch the rare earth tantalate ceramic block at a high temperature. The etching aid exists in the grain boundaries and preferentially reacts with the oxide molten salt, thereby being able to perform grain boundary etching on the rare earth tantalate ceramic block. After etching, clear grain boundaries can be observed, which is beneficial to studying the microstructure of the rare earth tantalate ceramic, such as the grain morphology, size, and ferroelastic domain.
[0043] (2) The method for etching the grain boundaries of rare earth tantalate ceramics provided by the present invention does not involve hazardous chemicals such as acids and alkalis and has strong applicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a cross-sectional morphology of the rare earth tantalate ceramic after grain boundary etching in Example 1;
[0045] Figure 2 This is a cross-sectional morphology of the rare earth tantalate ceramic after high-temperature thermal etching in Comparative Example 1. DETAILED DESCRIPTION
[0046] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0047] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0048] Example 1
[0049] This embodiment provides an etchant, comprising an oxide molten salt and Yb2Si2O7 sol, wherein the composition of the oxide molten salt is 33CaO-9MgO-13AlO 1.5-45SiO2. The oxide molten salt and Yb2Si2O7 sol are not mixed before use, but are packaged and placed separately.
[0050] The preparation method of the etchant is as follows:
[0051] 1. Preparation of oxide molten salt
[0052] (1) Weigh CaO, MgO, Al2O3 and SiO2 powders according to the composition of the oxide molten salt, and mix them evenly by wet ball milling. The wet ball milling uses anhydrous ethanol as the medium, the speed of the wet ball milling is 240r / min, and the time is 12h;
[0053] (2) The ball-milled slurry was placed in an oven at 80°C and dried for 12 h, and then passed through a 60-mesh sieve;
[0054] (3) placing the sieved mixed powder in a muffle furnace and sintering at 1200° C. for 24 hours to obtain molten salt;
[0055] (4) The molten salt was again wet-milled at 240 r / min for 12 h using anhydrous ethanol as a medium, and then dried in an oven at 80° C. for 12 h, and then passed through a 60-mesh sieve to obtain an oxide molten salt.
[0056] 2. Preparation of Yb2Si2O7 Sol as Etching Agent
[0057] Yb(NO3)3·5H2O and ethyl orthosilicate were dissolved in anhydrous ethanol and stirred for 1 hour to prepare Yb2Si2O7 sol. The molar ratio of Yb(NO3)3·5H2O to ethyl orthosilicate was 1:1.15, and the molar ratio of Yb(NO3)3·5H2O to anhydrous ethanol was 1:8.
[0058] This embodiment also provides a method for etching grain boundaries of rare earth tantalate ceramics, using the above-mentioned etchant for processing, comprising the following steps:
[0059] (1) immersing the yttrium tantalate powder in the Yb2Si2O7 sol in a volume ratio of 1:3, and vigorously shaking; after being fully wetted, centrifuging the turbid solution of the yttrium tantalate powder and the Yb2Si2O7 sol, and then discarding the upper layer of the Yb2Si2O7 sol to obtain wetted yttrium tantalate powder;
[0060] (2) placing the wetted yttrium tantalate powder obtained in step (1) in an oven at 80° C. and drying for 15 min; maintaining the dried yttrium tantalate powder at a pressure of 5 MPa for 1 min to complete cold pressing; and then maintaining the pressure at a pressure of 250 MPa for 15 min to complete the first cold isostatic pressing to obtain a preform;
[0061] (3) drying the preform obtained in step (2) in an oven at 80° C. for 24 h, and then drying in an oven at 120° C. for 12 h; maintaining the dried preform at a pressure of 250 MPa for 15 min, performing a second cold isostatic pressing, and obtaining a preform;
[0062] (4) The green body obtained in step (3) is placed in a muffle furnace and sintered at 1650°C for 20 hours to obtain a yttrium tantalate ceramic block; the oxide molten salt powder is mixed with anhydrous ethanol in a volume ratio of 2:1, and the mixture is evenly coated on the yttrium tantalate ceramic block with a coating amount of 35 mg / cm2; the yttrium tantalate ceramic block coated with the oxide molten salt is then placed in a muffle furnace and kept at 1300°C for 50 hours for high temperature grain boundary etching.
[0063] The cross-sectional morphology of the yttrium tantalate ceramic block after grain boundary etching is analyzed. The cross-sectional morphology of the rare earth tantalate ceramic after grain boundary etching is shown in FIG. Figure 1 As shown. Figure 1 It can be seen that clear grain boundaries can be observed after etching.
[0064] Comparative Example 1
[0065] Comparative Example 1 uses conventional high-temperature thermal etching to perform grain boundary etching. The specific process is as follows:
[0066] (1) holding the yttrium tantalate powder at a pressure of 5 MPa for 1 minute to complete cold pressing; then holding the powder at a pressure of 250 MPa for 15 minutes to complete cold isostatic pressing to obtain a green body;
[0067] (2) placing the green body obtained in step (1) in a muffle furnace and sintering it at 1650° C. for 20 hours to obtain a yttrium tantalate ceramic block; placing the yttrium tantalate ceramic block in a muffle furnace and keeping it at 1300° C. for 50 hours for high-temperature thermal corrosion.
[0068] The cross-sectional morphology of the yttrium tantalate ceramic block after high-temperature thermal corrosion is analyzed. The cross-sectional morphology of the rare earth tantalate ceramic after high-temperature thermal corrosion is shown in the figure. Figure 2 As shown. Figure 2 It can be seen that clear grain boundaries of yttrium tantalate ceramics cannot be observed, and the grain morphology and size inside the ceramics cannot be well observed.
Claims
1. A method for etching the grain boundaries of rare earth tantalate ceramics, using an etchant for treatment, It is characterized in that The following steps are involved: (1) soaking rare earth tantalate powder in an etching aid, centrifuging, and removing the upper layer of liquid to obtain wet rare earth tantalate powder; (2) drying the wetted rare earth tantalate powder obtained in step (1), cold pressing the powder into a shape; and then performing a first cold isostatic pressing to obtain a preform; (3) drying the preformed body prepared in step (2); and then performing a second cold isostatic pressing to obtain a green body; (4) sintering the green body prepared in step (3) to obtain a rare earth tantalate ceramic block; mixing an oxide molten salt with anhydrous ethanol, coating the mixture on the rare earth tantalate ceramic block, and then performing grain boundary etching; The etchant comprises an oxide molten salt and an etching aid, wherein the composition of the oxide molten salt is a CaO-b MgO-cAlO 1.5 -dSiO 2 , wherein a=25-40, b=5-15, c=10-25, d=35-55, and a+b+c+d=100; the etching aid comprises Yb 2 Si 2 O 7 .
2. The grain boundary etching method according to claim 1, It is characterized in that The composition of the oxide molten salt is a CaO-b MgO-c AlO 1.5 -dSiO 2 , where a=28~38, b=5~15, c=10~20, d=35~50, and a+b+c+d=100.
3. The grain boundary etching method according to claim 1 or 2, It is characterized in that The etching aid is Yb 2 Si 2 O 7 Sol.
4. The grain boundary etching method according to claim 1, It is characterized in that In step (1), the volume ratio of the rare earth tantalate powder to the etching aid is 1:2 to 1:
5.
5. The grain boundary etching method according to claim 1, It is characterized in that In step (2), the first cold isostatic pressing process is to maintain the pressure at 200-300 MPa for 10-20 min; in step (3), the second cold isostatic pressing process is to maintain the pressure at 200-300 MPa for 10-20 min.
6. The grain boundary etching method according to claim 1, It is characterized in that In step (4), the sintering process is to sinter the green body prepared in step (3) at 1550-1650° C. for 12-48 hours.
7. The grain boundary etching method according to claim 1, It is characterized in that In step (4), the volume ratio of the oxide molten salt to anhydrous ethanol is 3:1 to 1:2; during the coating process, the coating amount is 20 to 40 mg / cm 2 .
8. The grain boundary etching method according to claim 1, It is characterized in that In step (4), the grain boundary etching process is carried out at 1250-1500° C. for 5-100 hours.
Citation Information
Patent Citations
Method for evaluating high-temperature molten salt corrosion resistance of ceramic material
CN114526976A
CMAS-corrosion-resistant high-entropy ceramic material with small grain size and preparation method of CMAS-corrosion-resistant high-entropy ceramic material
CN114671675A
Process for producing nanorcrystalline composites
US20050255239A1
Protective coating for ceramic components
US20060099358A1