A cobalt-based composite material, preparation method thereof and application thereof
The non-metallic coating layer is formed by discharge plasma sintering and atomic vapor deposition, which solves the problem of low electron mobility of cobalt-based alloys, improves the conductivity and cycle performance of lithium-ion battery anode materials, and is suitable for lithium-ion battery anode materials.
Patent Information
- Application Number
- CN202310027831.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-01-09
AI Technical Summary
Cobalt-based alloys have low electron mobility and are not suitable as negative electrode materials for lithium-ion batteries, resulting in poor charge and discharge performance.
The alloy precursor material is prepared by discharge plasma sintering, and a non-metallic semiconductor material layer is deposited by atomic vapor deposition to form a non-metallic coating layer with high capacity and large specific surface area, which improves electron mobility and structural stability.
Significantly improves the conductivity, fast charging performance and cycle performance of cobalt-based composite materials, is suitable for lithium-ion battery anode materials, and enhances battery capacity and cycle stability.
Smart Images

Figure CN116005030B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermoelectric materials, and in particular to a cobalt-based composite material, a preparation method thereof and applications thereof. Background Art
[0002] For lithium-ion batteries, the mainstream negative electrode material graphite material can no longer meet the growing energy density requirements due to its relatively low theoretical specific capacity (372mAh / g). Therefore, the premise for further application of lithium-ion batteries is to prepare negative electrode materials with suitable operating voltage, excellent cycle performance and high energy density.
[0003] The specific capacity of cobalt-based composite materials (oxides, sulfides, phosphides and alloys) is as high as 700~1000mAh / g, which is 2~3 times that of graphite negative electrode. They are also widely available, stable and environmentally friendly. However, the electron mobility of cobalt-based alloys is low, and the charge and discharge performance of batteries made with them as negative electrode materials is poor.
[0004] How to improve the charge and discharge performance of this material is one of the hot topics in the current research field. Patent CN112652699A discloses a method for preparing LaF3-doped CoSb3 thermoelectric material with P / N type transition, which optimizes the thermoelectric performance by introducing LaF3, and can affect the semiconductor type of the thermoelectric material according to its doping amount.
[0005] Patent CN113735181A discloses an antimony cobalt sulfide-carbon composite nanorod and its preparation method and use, which adopts a solvent thermal synthesis combined with a high temperature calcination method to prepare a multi-level hierarchical structure electrode material composed of antimony cobalt sulfide nanorods, and obtains uniform carbon-coated antimony cobalt sulfide. This patent effectively improves the cycle performance and rate performance of the electrode material. Summary of the invention
[0006] The main purpose of the present invention is to provide a cobalt-based composite material, a preparation method thereof and an application thereof, so as to solve the problem that the electron mobility of cobalt-based alloys in the prior art is low and is not suitable for application in the negative electrode of lithium-ion batteries.
[0007] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a cobalt-based composite material is provided, and the preparation method comprises the following steps:
[0008] S1, subjecting a mixed powder of CoSb3 and graphitized carbon to spark plasma sintering, and then ball milling to obtain an alloy precursor material;
[0009] S2, using the alloy precursor material as a matrix, and depositing a non-metallic semiconductor material layer on the matrix by atomic vapor deposition to obtain a cobalt-based composite material.
[0010] Furthermore, the spark plasma sintering treatment is performed at a temperature of 300-500° C. and a time of 5-10 min. Preferably, the spark plasma sintering treatment is performed under an environment of a gas pressure of 50-80 MPa.
[0011] Further, in step S2, the atomic vapor deposition method includes:
[0012] Using non-metallic semiconductor materials as targets, first deposit for 1-3 seconds; then purge with inert gas for 50-70 seconds; then, introduce oxygen source for 4-8 seconds; then, purge with inert gas for 4-8 seconds; then introduce water for 0.03-0.07 seconds; finally, purge with inert gas for 40-80 seconds;
[0013] Repeat the above steps 10 to 100 times.
[0014] Furthermore, the volume ratio of CoSb3 to graphitized carbon is (99~95): (1~5).
[0015] Furthermore, the particle size of the alloy precursor material is 0.2-1.7 μm, and the deposition weight of the non-metallic semiconductor material layer is 1-5 g.
[0016] Furthermore, the non-metallic semiconductor is in granular form with a particle size of 100-200 nm; preferably, the non-metallic semiconductor includes one or more of silicon nanoparticles, boron nanoparticles, and selenium nanoparticles.
[0017] Furthermore, before step S1, the preparation method further comprises: pre-milling CoSb3 and graphitized carbon to obtain a mixed powder of CoSb3 and graphitized carbon; preferably, the particle size after pre-milling is 0.2-1.5 μm.
[0018] Furthermore, the graphitized carbon is one or more of carbon fiber, graphene, and natural graphite.
[0019] In order to achieve the above object, according to one aspect of the present invention, a cobalt-based composite material is provided, which is prepared by the above preparation method.
[0020] According to another aspect of the present invention, there is provided a use of the above-mentioned cobalt-based composite material in a negative electrode material for a lithium battery.
[0021] By applying the technical solution of the present invention, graphitized carbon is doped into CoSb3, and a non-metallic semiconductor layer is wrapped to form a cobalt-based composite material. On the one hand, CoSb3 contains octahedral voids that can accommodate filling atoms. The present invention forms p-type doping on it through carbon atoms, which generally increases its Fermi energy, causes carbon defects in the CoSb3 lattice, and thus improves its electron mobility, and has good electrical conductivity, fast charging performance and cycle performance. On the other hand, the present invention further forms a high-capacity, large-specific-surface-area non-metallic coating layer on the outer layer of the alloy precursor material, which can effectively prevent the cracking and oxidation of internal particles. In particular, the present invention uses a discharge plasma sintering technique to pre-form an alloy precursor material, and then uses an atomic vapor deposition method to deposit a non-metallic coating layer, which further improves the structural stability of the composite material, thereby facilitating the improvement of its cycle stability. Based on the above reasons, the cobalt-based composite material obtained by the preparation method of the present invention is very suitable as a negative electrode material for lithium-ion batteries, which can effectively increase the battery capacity and improve the battery cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0023] Figure 1 The SEM morphology of the cobalt-based composite material prepared according to Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0025] In order to solve the above problems in the prior art, according to one aspect of the present invention, a method for preparing a cobalt-based composite material is provided, and the preparation method comprises the following steps:
[0026] S1, subjecting a mixed powder of CoSb3 and graphitized carbon to spark plasma sintering, and then ball milling to obtain an alloy precursor material;
[0027] S2, using the alloy precursor material as a matrix, and depositing a non-metallic semiconductor material layer on the matrix by atomic vapor deposition to obtain a cobalt-based composite material.
[0028] By applying the technical solution of the present invention, graphitized carbon is doped into CoSb3, and a non-metallic semiconductor layer is wrapped to form a cobalt-based composite material. On the one hand, CoSb3 contains octahedral voids that can accommodate filling atoms. The present invention forms p-type doping on it through carbon atoms, which generally increases its Fermi energy, causes carbon defects in the CoSb3 lattice, and thus improves its electron mobility, and has good electrical conductivity, fast charging performance and cycle performance. On the other hand, the present invention further forms a high-capacity, large-specific-surface-area non-metallic coating layer on the outer layer of the alloy precursor material, which can effectively prevent the cracking and oxidation of internal particles. In particular, the present invention uses a discharge plasma sintering technique to pre-form an alloy precursor material, and then uses an atomic vapor deposition method to deposit a non-metallic coating layer, which further improves the structural stability of the composite material, thereby facilitating the improvement of its cycle stability. Based on the above reasons, the cobalt-based composite material obtained by the preparation method of the present invention is very suitable as a negative electrode material for lithium-ion batteries, which can effectively increase the battery capacity and improve the battery cycle performance.
[0029] Specifically, in the C-Co substitution state, the s orbital contribution of the carbon atom has a slight peak in the HOMO, so there is a similar gain contribution between the s orbital and the d orbital to the Fermi level; the contribution of the d orbital to the Fermi level is much greater than that of the s orbital; although similarly, due to the broken symmetry, the p orbital will also be delocalized from Sb, which causes a certain loss of contribution. However, considering all the above situations, the Fermi energy increases significantly overall.
[0030] On the other hand, in terms of preparation technology, the present invention deposits a non-metallic semiconductor material layer by atomic vapor deposition, so that when the cobalt-based composite material obtained by the present invention is used as a negative electrode material for lithium-ion batteries, it can effectively reduce the production of dendrites when lithium ions are embedded and de-embedded in the alloy, thereby improving the discharge specific capacity and initial charge and discharge efficiency of the material.
[0031] The SEM morphology of the cobalt-based composite material prepared according to the present invention is as follows: Figure 1 As shown. Figure 1 It can be seen that the cobalt-based composite material of the present invention has a granular structure, a uniform size distribution, and a particle size between 0.5 and 2 μm.
[0032] In a preferred embodiment, the spark plasma sintering treatment temperature is 300-500°C and the time is 5-10 minutes; preferably, the spark plasma sintering treatment is carried out under an environment with a gas pressure of 50-80 MPa. The spark plasma sintering treatment under the above preferred conditions is more conducive to doping the graphitized carbon material with the alloy, causing C-Co substitution to improve the conductivity of the composite material.
[0033] In order to further improve the cycle performance, in a preferred embodiment, in step S2, the atomic vapor deposition method includes:
[0034] The non-metallic semiconductor material is used as the target material, and is first deposited for 1 to 3 seconds; then purged with an inert gas for 50 to 70 seconds; then, an oxygen source is introduced for 4 to 8 seconds; then, an inert gas is purged for 4 to 8 seconds; then, water is introduced for 0.03 to 0.07 seconds; and finally, an inert gas is purged for 40 to 80 seconds;
[0035] Repeat the above steps 10 to 100 times.
[0036] Carrying out spark plasma sintering treatment according to the above preferred process is more conducive to improving the discharge capacity and the initial charge and discharge efficiency.
[0037] In actual operation, the above-mentioned inert gas includes but is not limited to nitrogen, argon and the like.
[0038] In order to further improve the conductivity, in a preferred embodiment, the volume ratio of CoSb3 to graphitized carbon is (99-95): (1-5). Doping CoSb3 with graphitized carbon according to the above volume ratio is more conducive to the combination of graphitized carbon material and alloy, improving the total contribution of Fermi energy and increasing the conductivity of the composite material, while also reducing the occurrence of side reactions between lithium ions and negative electrode materials and reducing the formation of lithium dendrites, thereby improving the cycle performance.
[0039] In a preferred embodiment, the particle size of the alloy precursor material is 15 μm, and the deposition weight of the non-metallic semiconductor material layer is 1 to 5 g. The above conditions are preferred to better prevent the expansion and cracking of the alloy particles, which is conducive to stabilizing the structure of the cobalt-based composite material.
[0040] In order to further improve the conductivity, in a preferred embodiment, the non-metallic semiconductor is granular with a particle size of 100-200 nm; preferably, the non-metallic semiconductor is one or more of silicon nanoparticles, boron nanoparticles, and selenium nanoparticles. The above common non-metallic semiconductors can well achieve the modification purpose of the present invention. In practical applications, silicon nanoparticles have a relatively better effect compared to other non-metallic semiconductors.
[0041] In order to make the spark plasma sintering treatment more complete, in a preferred embodiment, before step S1, the preparation method further includes: pre-milling CoSb3 and graphitized carbon to obtain a mixed powder of CoSb3 and graphitized carbon; preferably, the particle size after pre-milling is 0.5~2μm.
[0042] In order to further enhance the effect of graphitized carbon doping modification, in a preferred embodiment, the graphitized carbon is one or more of carbon fiber, graphene, and natural graphite.
[0043] According to another aspect of the present invention, a cobalt-based composite material prepared by the above-mentioned preparation method is provided. The material of the present invention has excellent electrical conductivity, conductivity, first discharge capacity, first efficiency, fast charging performance and cycle performance.
[0044] According to another aspect of the present invention, there is provided an application of the above-mentioned cobalt-based composite material in a lithium battery. The lithium-ion battery of the present invention has conductive properties, conductivity, initial discharge capacity, initial efficiency, fast charging performance and cycle performance.
[0045] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0046] Example 1
[0047] S1: 99.65 g CoSb3 and 0.35 g carbon fiber (CF) were added to a ball mill and ball-milled at 500 rpm for 1 hour. The mixed powder was transferred to a carbon mold and subjected to spark plasma sintering (SPS) at 300 °C for 10 min under vacuum at 50 MPa. The mixture was then placed in a ball mill and ball-milled to obtain a CoSb3-CF (1.5 vol%) precursor material.
[0048] S2: Using atomic vapor deposition, the alloy precursor material is transferred into a vacuum chamber and used as a substrate, and silicon nanoparticles are used as a target. Silicon nanoparticles are deposited on the alloy substrate according to the following parameters (① silicon nanoparticle material is deposited for 1 second; ② nitrogen purge for 60 seconds; ③ oxygen source is introduced for 5 seconds; ④ nitrogen purge for 5 seconds; ⑤ water is introduced for 0.05 seconds; ⑥ nitrogen purge for 50 seconds; ⑦ 45 cycles from step ①) to obtain a silicon nanoparticle-coated alloy composite material. The weight of the coating layer is 3g.
[0049] Example 2
[0050] S1: 99.3 g CoSb3 and 0.7 g graphene were added to a ball mill, and the mixed powder was transferred to a carbon mold after ball milling at 600 rpm for 1 hour. The mixed powder was subjected to spark plasma sintering (SPS) at 400 °C for 10 min under vacuum of 50 MPa, and then placed in a ball mill for ball milling to obtain a CoSb3-graphene (3 vol%) precursor material.
[0051] S2: Using atomic vapor deposition, the alloy precursor material is transferred into a vacuum chamber and used as a substrate, and boron nanoparticles are used as a target. Silicon nanoparticles are deposited on the alloy substrate according to the following parameters (① boron nanoparticles are deposited for 1 second; ② nitrogen purge for 50 seconds; ③ oxygen source is introduced for 4 seconds; ④ nitrogen purge for 4 seconds; ⑤ water is introduced for 0.03 seconds; ⑥ nitrogen purge for 40 seconds; ⑦ 70 cycles from step ①) to obtain a boron nanoparticle-coated alloy composite material. The weight of the coating layer is 4g.
[0052] Example 3
[0053] S1: 99.7 g CoSb3 and 0.3 g natural graphite were added to a ball mill and ball-milled at 400 rpm for 1 hour. The mixed milled composite powder was transferred to a carbon mold and subjected to spark plasma sintering (SPS) at 300 °C for 15 min under vacuum of 50 MPa. The mixture was then placed in a ball mill and ball-milled to obtain a CoSb3-natural graphite (1.2 vol%) precursor material.
[0054] S2: Using atomic vapor deposition, the alloy precursor material is transferred into a vacuum chamber and used as a substrate, and selenium nanoparticles are used as a target. Selenium nanoparticles are deposited on the alloy substrate according to the following parameters (① Selenium nanoparticle material deposition for 3 seconds; ② Nitrogen purge for 70 seconds; ③ Oxygen source for 8 seconds; ④ Nitrogen purge for 8 seconds; ⑤ Water for 0.07 seconds; ⑥ Nitrogen purge for 80 seconds; ⑦ 45 cycles from step ①) to obtain a selenium nanoparticle-coated alloy composite material. The weight of the coating layer is 4g.
[0055] Example 4
[0056] S1: 99.8 g CoSb3 and 0.2 g carbon fiber were added to a ball mill and ball milled at 500 rpm for 1 hour. The mixed powder was transferred to a carbon mold and subjected to spark plasma sintering (SPS) at 300 °C for 10 min under vacuum at 50 MPa. The mixture was then placed in a ball mill and ball milled to obtain a CoSb3-CF (0.9 vol%) precursor material.
[0057] S2: The prepared CoSb3-CF (0.9 vol%) precursor material is subjected to vapor deposition to obtain a silicon nanoparticle-coated alloy composite material according to step S2 of Example 1. The weight of the coating layer is 3 g.
[0058] Example 5
[0059] S1: 98.7 g CoSb3 and 1.3 g carbon fiber were added to a ball mill and milled at 500 rpm for 1 hour. The mixed powder was transferred to a carbon mold and subjected to spark plasma sintering (SPS) at 300 °C for 10 min under vacuum at 50 MPa. The mixture was then milled in a ball mill to obtain a CoSb3-CF (5.6 vol%) precursor material.
[0060] S2: The prepared CoSb3-CF (5.6 vol%) precursor material is subjected to vapor deposition to obtain a silicon nanoparticle-coated alloy composite material according to step S2 of Example 1. The weight of the coating layer is 3 g.
[0061] Example 6
[0062] The difference from Example 1 is that the added amounts of CoSb3 and carbon fiber are 99.75 g and 0.25 g CoSb3-CF (1.0 vol%), respectively.
[0063] Example 7
[0064] The difference from Example 1 is that the added amounts of CoSb3 and carbon fiber are 98.8 g and 1.2 g CoSb3-CF (5.0 vol%), respectively.
[0065] Example 8
[0066] The difference from Example 1 is that the spark plasma sintering temperature is 500° C., the vacuum is 80 MPa, and the sintering time is 5 min.
[0067] Example 9
[0068] The difference from Example 1 is that the mass of the coating layer of the silicon nanoparticles is 5 g. Example 10
[0069] The difference from Example 1 is that the mass of the coating layer of the silicon nanoparticles is 1 g.
[0070] Embodiment 11
[0071] The difference from Example 1 is that the mass of the coating layer of the silicon nanoparticles is 6 g.
[0072] Comparative Example 1
[0073] S1: Add CoSb3 to the ball mill, and after ball milling at 500 rpm for 1 hour, transfer 99.65g of CoSb3 to the vacuum chamber and use it as the substrate. Silicon nanoparticles are used as the target material. According to the following parameters (① silicon nanoparticle material for 1 second; ② nitrogen purge for 60 seconds; ③ oxygen source for 5 seconds; ④ nitrogen purge for 5 seconds; ⑤ water for 0.05 seconds; ⑥ nitrogen purge for 50 seconds; ⑦ 45 cycles from step ①), silicon nanoparticles are deposited on the alloy substrate to obtain a silicon nanoparticle-coated alloy material. The mass of the silicon nanoparticle coating layer is 3g.
[0074] Comparative Example 2
[0075] 99.65 g of CoSb3 and 0.35 g of carbon fiber were added to a ball mill and ball-milled at 500 rpm for 1 hour. The composite powder obtained by mixing and ball-milling was used as a precursor without spark plasma sintering. A composite material was obtained according to step 2 of Example 1.
[0076] Comparative Example 3
[0077] The CoSb3-CF (1.5 vol%) precursor material prepared in S1 in Example 1 was directly used as the negative electrode material.
[0078] Test method:
[0079] 1. SEM test: The alloy composite material prepared in Example 1 was subjected to SEM test. The test results are as follows: Figure 1 shown.
[0080] 2. Powder physicochemical properties test: The negative electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 3 were tested for tap density, specific surface area and specific capacity in accordance with GB / T24533-2019 “Graphite Negative Electrode Materials for Lithium Ion Batteries”. The results are shown in Table 1.
[0081] 3. Electrochemical performance test: The negative electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 3 were assembled into button cells. The assembly method is as follows: a binder, a conductive agent and a solvent are added to the negative electrode material, stirred and slurried, coated on a copper foil, and dried and rolled to obtain a negative electrode sheet. The button cell was assembled in a hydrogen-filled glove box, and the electrochemical performance test was carried out on a Wuhan Blue Electric CT2001A battery tester. The charge and discharge voltage range was 0.005V to 2.0V, and the charge and discharge rate was 0.1C. The test results are shown in Table 2.
[0082] 4. Soft pack battery test: The negative electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 3 were prepared into negative electrode sheets, with ternary materials (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) as the positive electrode, LiPF6 solution (solvent is EC+DEC, volume ratio is 1:1, LiPF6 concentration is 1.3 mol / L) as the electrolyte, and celegard2400 as the separator to prepare a 5Ah soft pack battery. Then the cycle performance and rate performance of the soft pack battery were tested.
[0083] Cycle performance test conditions: charge and discharge current 1C / 1C, voltage range 2.8~4.2V, cycle number 500 times.
[0084] Rate performance test conditions: charging rate: 1C / 3C / 5C / 8C, discharge rate 1C; voltage range: 2.8~4.2V.
[0085] The test results are shown in Tables 3 and 4.
[0086] Table 1
[0087] Table 2
[0088] Table 2 continued
[0089] Table 3
[0090] Table 4
[0091] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0092] It can be seen from Table 1 that the electrical conductivity of the composite materials prepared in the examples of the present invention is equivalent to or higher than that of the comparative examples, especially the electrical conductivities of Examples 1 to 11 are mostly maintained above 24 S / cm.
[0093] It can be seen from Table 2 that the first discharge capacity of the lithium ion battery prepared by the present invention can basically reach more than 400 mAh / g, and the first charge and discharge efficiency is more than 90%.
[0094] It can be seen from Table 3 that the cycle performance of the soft-pack battery prepared from the alloy material of the present invention is better than that of the comparative example. The reason is that in terms of 1C / 1C rate cycle performance, the non-metallic semiconductor wrapped in the outer layer can prevent the alloy particles from expanding and cracking, and stabilize the structure of the composite material; at the same time, the addition of graphitized carbon material can also improve its conductivity and reduce the occurrence of side reactions, thereby improving the cycle performance.
[0095] It can be seen from Table 4 that the soft-pack batteries prepared in Examples 1 to 11 of the present invention have a better constant current ratio and excellent cycle performance.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cobalt-based composite material, characterized in that: The preparation method comprises the following steps: S1, subjecting a mixed powder of CoSb3 and graphitized carbon to spark plasma sintering, and then ball milling to obtain an alloy precursor material; S2, using the alloy precursor material as a matrix, and depositing a non-metallic semiconductor material layer on the matrix by atomic vapor deposition to obtain the cobalt-based composite material; the non-metallic semiconductor is one or more of silicon nanoparticles, boron nanoparticles, and selenium nanoparticles; Wherein, the graphitized carbon is one or more of carbon fiber, graphene, and natural graphite; the particle size of the alloy precursor material is 0.2-1.7 μm, and the deposition weight of the non-metallic semiconductor material layer is 1-5 g.
2. The preparation method according to claim 1, characterized in that: The spark plasma sintering treatment is performed at a temperature of 300-500° C. and for a time of 5-10 minutes.
3. The preparation method according to claim 2, characterized in that: The spark plasma sintering process is performed under an environment with a gas pressure of 50-80 MPa.
4. The preparation method according to claim 1, characterized in that: In the step S2, the atomic vapor deposition method comprises: Using non-metallic semiconductor materials as targets, first deposit for 1-3 seconds; then purge with inert gas for 50-70 seconds; then, introduce oxygen source for 4-8 seconds; then, purge with inert gas for 4-8 seconds; then introduce water for 0.03-0.07 seconds; finally, purge with inert gas for 40-80 seconds; Repeat the above steps 10 to 100 times.
5. The preparation method according to any one of claims 1 to 3, characterized in that: The volume ratio of the CoSb3 to the graphitized carbon is (99~95):(1~5).
6. The preparation method according to any one of claims 1 to 3, characterized in that: Before the step S1, the preparation method further comprises: pre-ball milling the CoSb3 and the graphitized carbon to obtain a mixed powder of the CoSb3 and the graphitized carbon.
7. The preparation method according to claim 6, characterized in that: The particle size after the pre-ball milling treatment is 0.2-1.5 μm.
8. A cobalt-based composite material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the cobalt-based composite material according to claim 8 in negative electrode materials for lithium batteries.