A cemented carbide tool for cutting titanium alloy and a preparation method thereof

By using tungsten carbide-cobalt-nickel-aluminum cemented carbide in titanium alloy tools, Ni3Al intermetallic compounds are generated, tool wear and sticking problems in titanium alloy processing are solved, high-temperature hardness and bending strength are improved, and use is extended life.

CN116005058BActive Publication Date: 2024-11-05ZHEJIANG HENGCHENG CEMENTED CARBIDE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211578206.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-05
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The poor thermal conductivity of titanium alloy causes the tool to rise sharply during processing, the hardness decreases, and wear is accelerated. Due to the large affinity, the phenomenon of sticking the tool is severe, which reduces the service life of the tool. The strength of existing cemented carbide tools at high temperatures and The hardness is reduced and the impact resistance is insufficient, making it difficult to be suitable for rough processing of titanium alloys.

Method used

Tungsten carbide-cobalt-nickel-chromium-aluminum carbide is prepared by ball milling and sintering processes to produce Ni3Al intermetallic compounds precipitated in cobalt/nickel phase, strengthen the bonding phase, improve high temperature strength and hardness, and avoid intergranular brittleness. , extend the service life.

Benefits of technology

It significantly improves the high-temperature hardness and bending strength of the tool, extends the service life of the titanium alloy processing process, improves the cutting ability of titanium alloy, and improves the room temperature hardness and high-temperature hardness, and increases the flexural strength by more than 15%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116005058B_ABST
    Figure CN116005058B_ABST
Patent Text Reader

Abstract

The invention discloses a titanium alloy cutting cemented carbide tool, comprising the following components by mass fraction: 93-94% tungsten carbide, 3-4% cobalt, 2-3% nickel, 0.1-0.2% chromium, and 0.2-0.3% aluminum, and discloses a preparation method of the titanium alloy cutting cemented carbide tool. The alloy of the invention is composed of two bonding metal phases, namely, a cobalt / nickel phase and a Ni3Al intermetallic compound phase, and a tungsten carbide phase. The Ni3Al intermetallic compound phase is uniformly precipitated in the cobalt / nickel phase, thereby strengthening the strength of the cobalt / nickel phase and avoiding the intergranular brittleness problem of Ni3Al, thereby improving the high temperature hardness and strength of the alloy blade, while not reducing its overall impact resistance, thereby extending the service life of the titanium alloy processing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cemented carbide tool for cutting titanium alloy and a preparation method thereof. Background Art

[0002] The thermal conductivity of titanium alloy is poor, which is 1 / 6 of that of 45# steel. The high heat generated during the processing cannot be effectively diffused, and a large amount of heat is accumulated on the cutting edge. The temperature rises sharply, resulting in a decrease in the hardness of the blade, softening the blade, and easily accelerating tool wear. Titanium alloy also has a large affinity, and the tool sticking phenomenon is serious during the processing. The friction between the tool body and the workpiece is increased, resulting in a large amount of heat release, which reduces the service life of the tool.

[0003] Due to the above characteristics of titanium alloy, it is not possible to use hard alloys containing titanium carbide or blades containing titanium carbonitride coatings, which have a strong affinity with titanium alloys, in the titanium alloy processing process. At present, the blade grades commonly used in titanium alloy processing are WC-CO alloy blades such as YG6 / YG8.

[0004] Under high temperature conditions during the machining process, the strength and hardness of tungsten carbide-cobalt cemented carbide alloy decreases rapidly, the tool life is not high, and it is easy to wear prematurely, causing tool failure.

[0005] In the prior art, Ni3Al is also used as a bonding metal in titanium alloy cutting blades. Ni3Al has the advantages of high hardness, high oxidation resistance, high temperature red hardness, etc., but Ni3Al has intergranular brittleness and poor impact resistance. In the actual titanium alloy processing process, it can only be used in the cutting process requiring low impact applications such as finishing, but is not suitable for the roughing and semi-finishing processes of titanium alloys. Summary of the invention

[0006] The object of the present invention is to provide a cemented carbide cutting tool for titanium alloy machining with a bonding phase strengthened by an intermetallic compound, and a method for preparing the cemented carbide involved in realizing such a tool.

[0007] The technical solution adopted by the present invention is:

[0008] A cemented carbide tool for cutting titanium alloys, comprising the following components by mass fraction: 93-94% tungsten carbide, 3-4% cobalt, 2-3% nickel, 0.1-0.2% chromium, and 0.2-0.3% aluminum; preferably, the tool is composed of the following components by mass fraction: 93.7% tungsten carbide, 3.6% cobalt, 2.4% nickel, 0.1% chromium, and 0.2% aluminum.

[0009] The titanium alloy cutting cemented carbide tool is prepared by the following method:

[0010] (1) tungsten carbide, cobalt powder, nickel powder, high-purity aluminum nitride, and chromium carbide powder are mixed according to the component ratio, the obtained powder is added with a molding agent, and the mixture is ball-milled and mixed in a ball mill;

[0011] (2) After the ball milled slurry is dried, it is pressed into a green billet through a mold on a press, and the green billet is placed in a sintering furnace for sintering at a sintering temperature of 1460° C. to 1490° C., and then cooled to room temperature;

[0012] (3) The sintered alloy is subjected to a tempering heat treatment, heated to 600-900° C. and kept at this temperature for 10-11 hours, and then cooled to room temperature to obtain the cemented carbide tool for cutting the titanium alloy.

[0013] The present invention also provides a method for preparing the cemented carbide tool for cutting titanium alloy, the method comprising the following steps:

[0014] (1) tungsten carbide, cobalt powder, nickel powder, high-purity aluminum nitride, and chromium carbide powder are mixed according to the component ratio, the obtained powder is added to the molding agent, and the mixture is ball-milled in a ball mill for 20 to 30 hours;

[0015] The molding agent is refined paraffin wax, and the amount of refined paraffin wax is 1-2% of the mass of the powder;

[0016] The ball mill uses alcohol as a grinding medium with a solid-liquid ratio of 5 to 6:1;

[0017] The ball-to-material ratio of the ball mill is preferably 4 to 5:1;

[0018] (2) After the ball milled slurry is dried, it is pressed into a green billet through a mold on a press, and the green billet is placed in a sintering furnace for sintering at a temperature of 1460° C. to 1490° C. for 2 to 3 hours, and then cooled to room temperature;

[0019] Preferably, the sintering process is:

[0020] In a hydrogen atmosphere, heat to 400°C for 7 to 8 hours, keep warm for 1 to 2 hours, with a hydrogen flow rate of 40 to 60 L / min, use hydrogen to dewax, then evacuate to 20-50 Pa, heat to 1460°C-1490°C for 10 to 11 hours, perform vacuum sintering, then fill with argon to make the pressure reach 5 MPa, keep warm at 1460°C-1490°C for 2 to 3 hours, perform pressure sintering, and then cool to room temperature, preferably the cooling rate is >10°C / min, more preferably 11 to 30°C / min; more preferably the cooling rate is 15 to 20 / min;

[0021] (3) The sintered alloy is subjected to a tempering heat treatment, heated to 600-900° C. (preferably 700-800° C.) and kept at this temperature for 10-11 hours, and then cooled to room temperature to obtain the cemented carbide tool for cutting titanium alloy.

[0022] The particle size of the tungsten carbide, cobalt powder, nickel powder, high-purity aluminum nitride, and chromium carbide powder is preferably 1 to 10 μm, more preferably 1 to 2 μm, and more preferably 1.5 to 2 μm;

[0023] The present invention uses tungsten carbide-cobalt-nickel-chromium-aluminum elements to make an alloy, generates Ni3Al intermetallic compounds inside the alloy and precipitates in the cobalt / nickel phase, thereby strengthening the bonding phase. By virtue of the positive high temperature effect of Ni3Al intermetallic compounds at 600-800°C, the high temperature strength and hardness of the alloy blade are improved, and the service life of the titanium alloy processing process is extended.

[0024] The alloy of the present invention is composed of two bonding metal phases, namely, a cobalt / nickel phase and a Ni3Al intermetallic compound phase, and a tungsten carbide phase. Through high-temperature sintering, the three elements of Co, Ni and Al constituting the bonding metal phase are fully melted and uniformly mixed in the high-temperature liquid phase. Under rapid cooling conditions (greater than 10°C per minute), the three bonding metals first form a solid solution and cool to room temperature, and then undergo a tempering heat treatment at 600-900°C, so that part of Ni and Al in the solid solution generate a Ni3Al intermetallic compound phase and are uniformly precipitated in the cobalt / nickel phase. The precipitated Ni3Al intermetallic compound phase is uniform and fine, which greatly enhances the strength of the cobalt / nickel phase and avoids the intercrystalline brittleness problem of Ni3Al, so that the alloy blade has improved high-temperature hardness and strength without reducing its overall impact resistance.

[0025] The hard alloy tool for cutting titanium alloy produced by the present invention has a room temperature hardness of 90.5HRA and a hardness of 86.5HRA at 800°C, which is 9% higher than that of the YG6 tool in the prior art, and the bending strength is also significantly improved, which can be as high as 3000MPa, which is more than 15% higher than that of the YG6 tool in the prior art. The present invention significantly improves the high temperature strength and hardness of the tool, improves the cutting ability of the tool for titanium alloy, and prolongs the service life of the titanium alloy processing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Room temperature flexural strength curve of cemented carbide with different cobalt / nickel contents.

[0027] Figure 2 Room temperature flexural strength curve of cemented carbide with different aluminum content and sintering temperature.

[0028] Figure 3 Room temperature hardness curve of cemented carbide with different aluminum content and sintering temperature.

[0029] Figure 4 Metallographic photograph of the sample of Comparative Example 1.

[0030] Figure 5 Metallographic photograph of the sample of Example 3.

[0031] Figure 6 Metallographic photograph of the sample of Comparative Example 2.

[0032] Figure 7 Metallographic photograph of the sample of Example 4.

[0033] Figure 8 Electron microscope photograph of the sample of Example 4. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.

[0035] Example 1

[0036] Experimental study on binder phase composition (optimal cobalt / nickel content)

[0037] The composition of ordinary YG6 is WC-6%Co. WC-6%(Co+Ni) is taken as the research object, and Ni is added into the binder phase. The mass fraction of Ni in the binder (Co+Ni) is changed to 0%, 20%, 40%, 60%, and 100%, and the balance is cobalt. The preparation method is as follows:

[0038] Five samples of WC-6%Co, WC-(4.8%Co-1.2%Ni), WC-(3.6%Co-2.4%Ni), WC-(2.4%Co-3.6%Ni) and WC-6%Ni were mixed according to the composition ratio. The tungsten carbide particle size used was 1.5μm, the cobalt powder particle size was 1.5μm, and the nickel powder particle size was 1.5μm.

[0039] The five prepared samples were respectively placed in a ball mill and mixed evenly, with a ball-to-material ratio of 4:1, alcohol as the grinding medium, a solid-liquid ratio of 6:1, and a ball milling time of 30 hours.

[0040] The five mixed materials were dried and pressed into standard three-point bending cemented carbide transverse fracture strength B-type test strips, with five strips pressed for each test strip.

[0041] The sample strip is placed in a vacuum sintering furnace for sintering. The sintering process is as follows:

[0042] In a hydrogen atmosphere, heat to 400°C for 8 hours, keep warm for 1 hour, with a hydrogen flow rate of 40-60L / min, use hydrogen to dewax, then evacuate to 20-50pa, heat to 1460°C for 10-11 hours, perform vacuum sintering, then keep warm at 1460°C for 2 hours, fill with argon to make the pressure reach 5MPa, perform pressure sintering, then cool to room temperature, with a cooling rate of 15°C / min, perform tempering heat treatment on the sintered alloy, heat to 700°C and keep warm for 10 hours, cool to room temperature with the furnace, measure the strength of the prepared sample by three-point bending, measure the density by the watertight method, and measure the hardness by Rockwell hardness test.

[0043] After sintering, the room temperature flexural strength of fully dense samples WC-6%Co, WC-(4.8%Co-1.2%Ni), WC-(3.6%Co-2.4%Ni), WC-(2.4%Co-3.6%Ni) and WC-6%Ni are as follows: Figure 1 As shown. Figure 1 It can be seen that with the increase of Ni content, the strength of WC-(Co+Ni) cemented carbide reaches its maximum value when the binder is 60% Co-40% Ni. This is because an appropriate amount of nickel can stabilize the face-centered cubic cobalt phase at room temperature, thereby strengthening it.

[0044] Therefore, the Co content is preferably 3.6% and the Ni content is preferably 2.4%.

[0045] Example 2

[0046] Trace element aluminum and sintering parameter optimization to improve high temperature hardness and strength

[0047] Trace element aluminum is added to the raw materials. At an appropriate sintering temperature, the aluminum element and the nickel element in the bonding phase form the intermetallic compound AlNi3, which strengthens the bonding phase performance and enhances the high-temperature hardness and strength of the alloy product.

[0048] WC-(3.6%Co-2.4%Ni) was used as the research object, wherein the mass fraction of aluminum added to the binder varied from 0%, 0.1%, 0.2%, 0.3%, and 0.4%. After the addition of aluminum, the mass fraction of tungsten carbide decreased accordingly with the addition of aluminum. The aluminum was added in the form of 2μm high-purity aluminum nitride, which can be dispersed evenly and avoid aluminum oxidation. The preparation method is the same as that of Example 1, except that the pressure sintering temperatures are 1400°C, 1430°C, 1460°C, 1490°C, and 1520°C, respectively. The strength of the prepared samples was measured by three-point bending, the density was measured by the watertight method, and the hardness was measured by the Rockwell hardness test.

[0049] The room temperature flexural strength of the fully dense sample obtained after sintering is as follows Figure 2 As shown, the room temperature hardness is Figure 3 As shown. Figure 2It can be seen that with the increase of Al content, the strength of the test block reaches the maximum value when the Al content is 0.2% and the sintering temperature is 1490℃. In the range of 0.2%-0.3%, the sintering temperature is 1460℃-1490℃, which is at a relatively high level. This is because the appropriate amount of aluminum and nickel generate intermetallic compounds at a sintering temperature above 1450℃, thereby strengthening the bonding phase and improving the strength of the alloy. Excessive temperature will cause the cemented carbide to be overburned, deformed, and the bonding phase will precipitate, resulting in a decrease in strength. Excessive aluminum content will produce too much AlNI3 in the alloy, causing the material to become more brittle and affecting the material's bending strength.

[0050] like Figure 3 As shown in the figure, with the increase of aluminum content, the hardness of WC-(3.6%Co-2.4%Ni) cemented carbide increases. This is mainly because with the increase of aluminum element, the proportion of AlNI3 in the bonding phase increases and the hardness of the test block increases.

[0051] Therefore, it can be concluded from the test data that the material properties reach the optimum when the aluminum content is 0.2% and the sintering temperature is 1490°C.

[0052] Example 3

[0053] The cemented carbide raw material was prepared according to Table 1, and the sample was prepared according to the steps of Example 1, with the pressure sintering temperature being 1490° C. The chromium element was added in the form of chromium carbide powder with a particle size of 1.5 μm.

[0054] Table 1

[0055]

[0056] The prepared samples were tested for strength by three-point bending, density by watertight method and hardness by Rockwell hardness test. The physical properties comparison of YG6 is shown in Table 2.

[0057] Table 2 Material physical properties:

[0058]

[0059] As shown in Table 2, the high temperature hardness of Example 3 is 9% higher than that of YG6, and the bending strength is also significantly improved, up to 3000MPa, which is more than 15% higher than that of the YG6 tool in the prior art. Compared with the sample of Comparative Example 1 without adding chromium element, the high temperature hardness of Example 3 is improved, and the metallographic photographs of Comparative Example 1 and Example 3 are as follows: Figure 4 , Figure 5 As shown, Figure 4It can be seen that in comparative example 1, the metallographic photograph without adding chromium element has more tungsten carbide thickening phenomenon, while in Example 3, due to the addition of chromium element, the tungsten carbide thickening phenomenon is significantly reduced. It can be seen that the addition of chromium element can significantly improve the tungsten carbide thickening phenomenon, and greatly avoid the blade fracture and failure caused by the transgranular fracture of coarse tungsten carbide during tool processing and application. The present invention introduces intermetallic compounds to precipitate in the cobalt / nickel phase to strengthen the cemented carbide bonding phase, significantly improves the high temperature strength and hardness of the tool, improves the tool's cutting ability for titanium alloys, and prolongs the service life of the titanium alloy processing process.

[0060] Example 4

[0061] The samples were prepared according to the raw material ratio and steps of Example 3, except that in Example 4, the sintering process was:

[0062] The sintering process is:

[0063] In a hydrogen atmosphere, heat to 400°C for 8 hours, keep warm for 1 hour, with a hydrogen flow rate of 40-60L / min, use hydrogen to dewax, then evacuate to 20-50pa, heat to 1460°C for 10-11 hours, perform vacuum sintering, then keep warm at 1490°C for 2 hours, fill with argon to make the pressure reach 5MPa, perform pressure sintering, then cool to room temperature, with a cooling rate of 15°C / min, and perform tempering heat treatment on the sintered alloy, heat to 800°C and keep warm for 10 hours, and cool to room temperature with the furnace.

[0064] The raw material ratio and steps of Comparative Example 2 are the same as those of Example 4, except that after sintering at 1490° C., the temperature is cooled to room temperature along with the furnace, and the cooling rate is about 5° C. / min.

[0065] The metallographic photographs of the samples obtained in Comparative Example 2 and Example 4 are as follows: Figure 6 , 7 As shown, the electron microscope photo of the sample of Example 4 is as follows Figure 8 shown.

[0066] Figure 6 It can be seen that under the condition of cooling rate of 5℃ per minute, Ni3Al phase aggregates, such as Figure 6 The black phase in the graph represents the aggregated Ni3Al phase. At a faster cooling rate, Figure 7 As shown, Figure 7 There is no black phase and no aggregation of Ni3Al phase.

[0067] In addition, under the conditions of rapid cooling (cooling to room temperature at >10°C per hour) and tempering at 800°C for 10 hours, the Ni3Al phase precipitates in nanometer size and is evenly distributed in the cobalt phase. Figure 8The electron microscope photo shows that the Ni3Al phase of about 100 nanometers is uniformly precipitated in the cobalt phase in the electron microscope photo. The size is very uniform and there is no large aggregation. This greatly enhances the strength of the cobalt / nickel phase.

[0068] The samples prepared in Example 4 and Comparative Example 2 were tested for strength by three-point bending, density by watertight method, and hardness by Rockwell hardness test. The physical property comparison is shown in Table 3.

[0069] Table 3 Material physical properties:

[0070]

[0071] As shown in Table 3, rapid cooling improves the hardness at room temperature and 800℃, as well as the bending strength. The coercive force is also significantly improved.

Claims

1. A method for preparing a cemented carbide tool for cutting titanium alloy, characterized in that The method comprises the following steps: (1) Tungsten carbide, cobalt powder, nickel powder, high-purity aluminum nitride, and chromium carbide powder are mixed according to a component ratio, and the obtained powder is mixed with refined paraffin by ball milling; the cemented carbide tool for titanium alloy cutting comprises the following components by mass fraction: tungsten carbide 93-94%, cobalt 3-4%, nickel 2-3%, chromium 0.1-0.2%, and aluminum 0.2-0.3%; (2) After the ball milled slurry is dried, it is pressed into a green billet through a mold on a press, and the green billet is placed in a sintering furnace for sintering at a temperature of 1460°C-1490°C, kept at this temperature for 2-3 hours, and then cooled to room temperature; the cooling rate is >10°C / min; (3) The sintered alloy is subjected to a tempering heat treatment, heated to 600-900° C. and kept at this temperature for 10-11 hours, and then cooled to room temperature to obtain the cemented carbide tool for titanium alloy cutting.

2. The method according to claim 1, characterized in that The titanium alloy cutting cemented carbide tool is composed of the following components by mass fraction: Tungsten carbide 93.7%, cobalt 3.6%, nickel 2.4%, chromium 0.1%, aluminum 0.2%.

3. The method according to claim 1, characterized in that In step (2), the sintering process is: Under hydrogen atmosphere, heat to 400℃ for 7~8 hours, keep warm for 1~2 hours, with a hydrogen flow rate of 40~60L / min, use hydrogen to dewax, then evacuate to 20-50pa, heat to 1460℃-1490℃ for 10~11 hours, perform vacuum sintering, then fill with argon to make the pressure reach 5~6MPa, keep warm at 1460℃-1490℃ for 2~3 hours, perform pressure sintering, and then cool to room temperature.

4. The method according to claim 1, characterized in that In step (1), the particle size of the tungsten carbide, cobalt powder, nickel powder, high-purity aluminum nitride, and chromium carbide powder is 1-10 μm.

5. The method according to claim 1, characterized in that In step (1), the ball milling time is 20 to 30 hours.

6. The method according to claim 1, characterized in that In step (1), the amount of refined paraffin wax is 1-2% of the mass of the powder.

7. The method according to claim 1, characterized in that In step (3), the tempering temperature is 700-800°C.

8. A cemented carbide tool for cutting titanium alloy prepared by the method according to any one of claims 1 to 7.

9. Use of the cemented carbide tool for cutting titanium alloy as claimed in claim 8 in cutting titanium alloy.

Citation Information

Cited By

  • Low-cost high-yield-strength free-cutting titanium alloy and preparation method thereof

    CN121428341A