A method for forming a composite SEI film in a lithium-ion battery
By pre-coating the surface of the negative electrode or separator of a lithium-ion battery with an inorganic lithium salt film and combining it with the SEI film formed during the formation process, the problem of positive electrode lithium source consumption during the formation process of lithium-ion batteries is solved, thereby improving the first charge-discharge efficiency and cycle life of the battery.
Patent Information
- Application Number
- CN202111521784.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-13
AI Technical Summary
Existing lithium-ion batteries consume nearly 10% of the lithium source in the cathode during the formation process, affecting the battery's cycle life. Furthermore, lithium replenishment technology is complex to operate and carries the risk of thermal runaway.
An inorganic lithium salt film composed of LiF, LiOH and Li2CO3 is pre-coated on the surface of the negative electrode or separator. The film is then combined with a chemically formed SEI film through a formation process to form a composite SEI film.
It reduces the consumption of active lithium in the cathode material, improves the first charge-discharge efficiency and battery cycle life, and simplifies the operation process.
Smart Images

Figure CN116014351B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to a method for forming a composite SEI film in a lithium ion battery. Background Art
[0002] As an important chemical power source, lithium-ion batteries are widely used in our daily lives due to their high energy density, excellent rate and power performance, long cycle life, safety and environmental protection. Currently, commercially produced lithium-ion batteries are generally composed of a positive electrode, a negative electrode, a separator and an electrolyte, in which the electrolyte can form a stable SEI film on the surface of the electrode material, especially the surface of the negative electrode material, during the initial formation and charging process.
[0003] The SEI film is an interfacial layer that has the characteristics of a solid electrolyte and is an electronic insulator. + Excellent conductor, Li + Insertion and extraction are possible freely through the passivation layer.
[0004] At present, the formation of SEI film is basically formed in the formation stage or by lithium replenishment technology. Generally, a dense SEI film is formed at the negative electrode of the battery by adjusting the formation voltage and formation current, thereby improving the cycle life of the battery. By using lithium replenishment technology, when the negative electrode material of the battery is formed into a film, the pre-lithiated lithium is preferentially consumed to form a film, thereby improving the battery cycle capacity.
[0005] CN110034336A discloses a battery formation method for forming a stable SEI film. The battery formation method comprises the following steps: (1) applying voltage to the electrodes of the battery to be formed and performing linear scanning to obtain a battery with a pre-constructed SEI film; (2) reforming the SEI film of the battery with the pre-constructed SEI film in step (1) to obtain a battery with a reformed SEI film; (3) applying voltage to the electrodes of the battery with the reformed SEI film in step (2) and performing linear scanning to obtain a formed battery.
[0006] CN109802109A discloses a method for pre-lithiation of a silicon-based negative electrode of a battery and simultaneously forming an SEI film, using silicon oxide, inert lithium powder, and 1-fluorodecane as raw materials and an organic solvent as a solvent to achieve pre-lithiation of the silicon-based negative electrode and simultaneously form an artificial SEI film.
[0007] The above scheme adopts the formation of SEI film during the formation process or the lithium replenishment technology, which preferentially consumes the pre-lithiated lithium to form the film when the battery negative electrode material forms the film. However, the formation of SEI film during the formation process consumes nearly 10% of the lithium source of the positive electrode, resulting in a decrease in the initial charge and discharge rate of the battery, affecting the subsequent cycle life of the battery. The pre-lithiation technology has high requirements on equipment and environment, and the process operation is relatively complicated. There is a greater risk of thermal runaway in the production process. Therefore, it is very necessary to develop a simple SEI film formation method that avoids consuming the positive electrode lithium source. Summary of the invention
[0008] The purpose of the present invention is to provide a method for forming a composite SEI film. The present invention first forms a thin SEI film on the surface of the negative electrode or the separator in a physical way, and then closely combines with the chemically formed SEI film after formation, so as to achieve the purpose of improving the initial efficiency of the battery cell.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] The present invention provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0011] mixing LiF, LiOH and Li2CO3 with a binder solution to obtain a mixed solution;
[0012] The mixed solution is coated on the surface of the negative electrode plate and / or the separator to obtain a negative electrode plate with a lithium salt film and / or a separator with a lithium salt film;
[0013] The negative electrode plate with lithium salt film and / or the separator with lithium salt film and the positive electrode plate are made into a battery cell. After formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0014] The present invention pre-coats an inorganic lithium salt composed of LiF, LiOH and Li2CO3 on the negative electrode plate or the separator to form a sparse ultra-thin film. During battery formation, the SEI film formed on the surface of the negative electrode combines with the above lithium salt to form a complete composite SEI film, which can reduce the consumption of active lithium in the positive electrode material and improve the initial charge and discharge efficiency.
[0015] Preferably, the mass ratio of LiF, LiOH and Li2CO3 is (1-1.5):(0.8-1.2):(0.8-1.2), for example: 1:0.8:0.8, 1.1:1:1, 1.2:1.1:1.2, 1:1:1 or 1.5:1.2:1.2, etc.
[0016] Preferably, when the mixed solution is coated on the surface of the diaphragm, the mixed solution is coated on the side of the diaphragm close to the negative electrode plate.
[0017] Since the diaphragm has abundant voids, the present invention coats the mixed inorganic lithium salt on the diaphragm and winds or stacks the diaphragm so that the side containing the lithium salt faces the negative electrode, which can reduce the consumption of active lithium in the positive electrode material and improve the initial charge and discharge efficiency.
[0018] Preferably, the solute of the binder solution includes PVDF and / or SBR;
[0019] Preferably, the solvent of the binder solution includes N-methylpyrrolidone.
[0020] Preferably, the mass concentration of the binder solution is 30-45%, for example, 30%, 32%, 35%, 40% or 45%.
[0021] Preferably, based on the mass of the mixed solution being 100%, the total mass fraction of LiF, LiOH and Li2CO3 is 1-6%, for example, 1%, 2%, 3%, 4%, 5% or 6%.
[0022] Preferably, the coating method comprises gravure coating and / or spray coating.
[0023] The present invention achieves the expected effect by adopting the gravure technology and the spraying technology, has low operation difficulty and simple process, and can also reduce the wetting time of the pole piece.
[0024] Preferably, the thickness of the lithium salt film is 100-300 nm, for example, 100 nm, 150 nm, 200 nm, 250 nm or 300 nm.
[0025] Preferably, the positive electrode plate comprises a lithium iron phosphate positive electrode plate.
[0026] Preferably, the formation includes one-step formation, two-step formation and three-step formation.
[0027] Preferably, the one-step formation ratio is 0.04 to 0.06C, for example, 0.04C, 0.045C, 0.05C, 0.055C or 0.06C, etc., the one-step formation vacuum degree is -40 to -50kPa, for example, -40kPa, -42kPa, -45kPa, -48kPa or -50kPa, etc., the one-step formation termination voltage is 3.4V, and the one-step formation protection voltage is 0 to 3.45V, for example, 0V, 0.5V, 1V, 2V, 3V or 4.5V, etc.
[0028] Preferably, the ratio of the two-step formation is 0.04 to 0.06C, for example: 0.04C, 0.045C, 0.05C, 0.055C or 0.06C, etc., the vacuum degree of the two-step formation is -40 to -50kPa, for example: -40kPa, -42kPa, -45kPa, -48kPa or -50kPa, etc., the termination voltage of the two-step formation is 3.4V, and the protection voltage of the two-step formation is 2 to 3.45V, for example: 2V, 2.5V, 2.8V, 3V or 4.5V, etc.
[0029] Preferably, the two-step formation is followed by a vacuum release treatment.
[0030] Preferably, the ratio of the three-step formation is 0.25-0.35C, for example: 0.25C, 0.27C, 0.3C, 0.32C or 0.35C, etc., the vacuum degree of the three-step formation is -75--85kPa, for example: -75kPa, -78kPa, -80kPa, -82kPa or -85kPa, etc., the termination voltage of the one-step formation is 3.5V, and the protection voltage of the three-step formation is 2.8-3.5V, for example: 2.8V, 3V, 3.2V, 3.4V or 3.5V, etc.
[0031] The chemical formation methods of the present invention are all carried out under strong vacuum conditions, which can ensure that the inorganic lithium salt can better combine with the SEI film formed during the chemical formation process to form a new SEI film.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The present invention pre-coats an inorganic lithium salt on the negative electrode plate or separator by a physical method. During the battery formation process, the SEI formed by an electrochemical method will combine with the physically coated lithium salt to form a new SEI film. At this time, the amount of positive electrode active material consumed by the formed SEI film is reduced, thereby improving the initial charge and discharge efficiency.
[0034] (2) The first charge efficiency of the battery containing the composite SEI film of the present invention can reach more than 94.11%, and the capacity retention rate after 500 cycles can reach more than 95.1%. By adjusting the addition ratio of the lithium source, the first charge efficiency can reach more than 98%, and the capacity retention rate after 500 cycles can reach more than 96%. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic diagram of the preparation process of the composite SEI film described in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0037] Example 1
[0038] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0039] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:1:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0040] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0041] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0042] The method flow chart of forming a composite SEI film is as follows Figure 1 shown.
[0043] Example 2
[0044] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0045] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.3:1.2:1.1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 4%;
[0046] (2) applying the mixed solution to the surface of the diaphragm electrode by gravure coating to form a diaphragm with a lithium salt film having a thickness of 200 nm;
[0047] (3) The separator with the lithium salt film is wound with the negative electrode plate and the acid lithium iron positive electrode plate to form a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45kPa for 24min, and the lower limit of the formation protection voltage is 0V and the upper limit is 3.45V. A two-step formation is carried out at a rate of 0.05C at -45kPa for 24min, and the lower limit of the formation protection voltage is 2V and the upper limit is 3.45V. After the vacuum is released, the vacuum is evacuated to -80kPa again, and the formation is carried out at 0.3C for 78min, and the lower limit of the formation protection voltage is 2.8V and the upper limit is 3.5V. The lithium salt film of the separator is close to the negative electrode side. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film, thereby obtaining a lithium ion battery.
[0048] Example 3
[0049] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0050] (1) mixing LiF, LiOH and Li2CO3 at a mass ratio of 0.8:1:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0051] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0052] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0053] Example 4
[0054] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0055] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.6:1:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0056] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0057] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C for 24 minutes at -45 kPa, and the lower limit of the formation protection voltage is 0 V, and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C for 24 minutes at -45 kPa, and the lower limit of the formation protection voltage is 2 V, and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V, and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film, and a lithium ion battery is obtained.
[0058] Example 5
[0059] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0060] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:0.6:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0061] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0062] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0063] Example 6
[0064] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0065] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:1.5:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0066] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0067] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0068] Example 7
[0069] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0070] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:1:0.6 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0071] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0072] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0073] Example 8
[0074] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0075] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:1:1.5 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0076] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 150 nm;
[0077] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0078] Example 9
[0079] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0080] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:1:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0081] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 50 nm;
[0082] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0083] Example 10
[0084] This embodiment provides a method for forming a composite SEI film in a lithium ion battery, the method comprising the following steps:
[0085] (1) mixing LiF, LiOH and Li2CO3 in a mass ratio of 1.2:1:1 with a PVDF solution having a mass concentration of 40% to obtain a mixed solution having a lithium salt mass concentration of 3%;
[0086] (2) applying the mixed solution to the surface of the negative electrode plate by gravure coating to form a negative electrode plate with a lithium salt film having a thickness of 400 nm;
[0087] (3) The negative electrode plate with the lithium salt film, the lithium iron phosphate positive electrode plate and the separator are made into a battery cell, and a one-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 0 V and the upper limit is 3.45 V. A two-step formation is carried out at a rate of 0.05C at -45 kPa for 24 minutes, and the lower limit of the formation protection voltage is 2 V and the upper limit is 3.45 V. After the vacuum is released, the vacuum is evacuated to -80 kPa again, and the formation is carried out at 0.3C for 78 minutes, and the lower limit of the formation protection voltage is 2.8 V and the upper limit is 3.5 V. After the formation, the SEI film on the surface of the negative electrode combines with the lithium salt to form a composite SEI film to obtain a lithium ion battery.
[0088] Comparative Example 1
[0089] The only difference between this comparative example and Example 1 is that no lithium salt coating is applied, and other conditions and parameters are exactly the same as those in Example 1.
[0090] Comparative Example 2
[0091] The only difference between this comparative example and Example 1 is that LiF is not added to the lithium salt coating, and other conditions and parameters are exactly the same as those in Example 1.
[0092] Comparative Example 3
[0093] The only difference between this comparative example and Example 1 is that LiOH is not added to the lithium salt coating, and other conditions and parameters are exactly the same as those in Example 1.
[0094] Comparative Example 4
[0095] The only difference between this comparative example and Example 1 is that Li2CO3 is not added to the lithium salt coating, and the other conditions and parameters are exactly the same as those in Example 1.
[0096] Performance Test:
[0097] The formed batteries obtained in Examples 1-10 and Comparative Examples 1-4 were tested for their initial charge and discharge efficiency and the capacity retention rate of the battery cells at 25°C 1C. The test results are shown in Table 1:
[0098] Table 1
[0099]
[0100]
[0101] As can be seen from Table 1 and Examples 1-10, the first charge efficiency of the battery containing the composite SEI film of the present invention can reach more than 94.11%, and the capacity retention rate after 500 cycles can reach more than 95.1%. By adjusting the addition ratio of the lithium source, the first charge efficiency can reach more than 98%, and the capacity retention rate after 500 cycles can reach more than 96%. After the three lithium salts are added, the first charge and discharge efficiency of the battery cell is greatly improved. Among them, the appropriate addition of LiF, LiOH, and Li2CO3 can not only improve the first charge and discharge efficiency of the battery cell but also improve the battery cell cycle capacity retention rate to a certain extent. However, when it exceeds a certain range, as the amount of the three increases, the battery cell cycle performance decreases. It is speculated that this may be because as the lithium salt increases, the internal resistance of the battery cell increases, resulting in a decrease in the battery cell cycle capacity. When it is below a certain range, the amount of the three has little effect on the first charge and discharge efficiency, and the improvement on the cycle is small.
[0102] By comparing Example 1 and Examples 3-8, it can be seen that the mass ratio of LiF, LiOH and Li2CO3 in the lithium salt coating will affect the performance of the SEI film. The mass ratio of LiF, LiOH and Li2CO3 is controlled within (1-1.5):(0.8-1.2):(0.8-1.2), and the SEI film is better. If it exceeds this range, although the first efficiency is improved to a certain extent, it will lead to an increase in the internal resistance of the battery cell and cause a decrease in the cycle performance.
[0103] By comparing Example 1 with Examples 9-10, it can be seen that the thickness of the lithium salt film in step (2) affects the performance of the SEI film. When the thickness of the lithium salt film is controlled at 100-300 nm, the SEI film has better performance. If the thickness of the lithium salt film is too thin, the improvement of the first charge and discharge efficiency of the battery cell will not be obvious, but its cycle performance will not be affected. If the thickness of the lithium salt film is too thick, although the first charge and discharge efficiency of the battery cell can be improved, the internal resistance of the battery cell will be increased, affecting the cycle performance of the battery cell.
[0104] By comparing Example 1 with Comparative Example 1, it can be seen that the present invention pre-coats an inorganic lithium salt on the negative electrode plate or the separator to form a sparse ultra-thin film. During battery formation, the SEI film formed on the surface of the negative electrode combines with the above-mentioned lithium salt to form a complete composite SEI film, which can reduce the consumption of active lithium in the positive electrode material and improve the initial charge and discharge efficiency.
[0105] By comparing Example 1 with Comparative Examples 2-4, it can be seen that the inorganic lithium salt film composed of LiF, LiOH and Li2CO3 can form a composite SEI film with the SEI film formed by an electrochemical method. The SEI film formed by this method has the best effect and the battery has the best initial charge and discharge efficiency.
[0106] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for forming a composite SEI film in a lithium-ion battery, It is characterized in that The method comprises the following steps: LiF, LiOH and Li 2 CO 3 mixing with a binder solution to obtain a mixed solution; LiF, LiOH and Li 2 CO 3 The mass ratio is (1~1.5):(0.8~1.2):(0.8~1.2); The mixed solution is coated on the surface of the negative electrode plate and / or the separator to obtain the negative electrode plate with the lithium salt film and / or the separator with the lithium salt film; When the mixed solution is coated on the surface of the diaphragm, the mixed solution is coated on the side of the diaphragm close to the negative electrode plate; The negative electrode sheet with lithium salt film and / or the separator with lithium salt film and the positive electrode sheet are made into a battery cell, and the SEI film on the surface of the negative electrode is formed with LiF, LiOH and Li 2 CO 3 Combined to form a composite SEI film, a lithium-ion battery is obtained; The chemical formation includes one-step chemical formation, two-step chemical formation and three-step chemical formation; The magnification of the one-step formation is 0.04~0.06C, the vacuum degree of the one-step formation is -40~-50kPa, the termination voltage of the one-step formation is 3.4V, and the protection voltage of the one-step formation is 0~3.45V; The ratio of the two-step formation is 0.04~0.06C, the vacuum degree of the two-step formation is -40~-50kPa, the termination voltage of the two-step formation is 3.4V, and the protection voltage of the two-step formation is 2~3.45V; After the two-step formation, vacuum release treatment is performed; The ratio of the three-step formation is 0.25-0.35C, the vacuum degree of the three-step formation is -75--85kPa, the termination voltage of the one-step formation is 3.5V, and the protection voltage of the three-step formation is 2.8-3.5V.
2. The method according to claim 1, It is characterized in that The solute of the binder solution includes PVDF and / or SBR.
3. The method according to claim 1, It is characterized in that The solvent of the binder solution includes N-methylpyrrolidone.
4. The method according to claim 1, It is characterized in that The mass concentration of the binder solution is 30-45%.
5. The method according to claim 1, It is characterized in that Taking the mass of the mixed solution as 100%, the LiF, LiOH and Li 2 CO 3 The total mass fraction is 1~6%.
6. The method according to claim 1, It is characterized in that The coating method includes gravure coating and / or spray coating.
7. The method according to claim 1, It is characterized in that The thickness of the lithium salt film is 100-300 nm.
8. The method according to claim 1, It is characterized in that The positive electrode plate includes a lithium iron phosphate positive electrode plate.