A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles

The preparation of carbon microsphere composite materials with loaded magnetic nanoparticles through simple mechanical mixing and high-temperature calcination has solved the problem of poor absorption performance of carbon-based composite materials in the prior art, and achieved a wider spectrum of electromagnetic wave absorption and attenuation effect.

CN116022773BActive Publication Date: 2024-11-26ZHENGZHOU UNIVERSITY OF AERONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211415850.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-11-26
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

In the field of electromagnetic wave absorption, existing carbon-based composite materials have problems such as complex preparation process and poor absorption performance, especially the large density and poor dispersion of magnetic nanoparticles, resulting in poor electromagnetic wave absorption performance.

Method used

A carbon microsphere composite material supported by magnetic nanoparticles is prepared by simple mechanical mixing and high-temperature calcining process. Through the high-temperature reaction of graphite phase carbon nitride and metal salt, a carbon microsphere supported magnetic nanoparticle composite is formed to improve wave absorption performance.

Benefits of technology

A wider effective absorption frequency band and stronger reflection loss value are achieved, which significantly improves the absorption performance. The preparation method is simple and safe, with good impedance matching performance and electromagnetic wave attenuation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116022773B_ABST
    Figure CN116022773B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a carbon microsphere composite material loaded with magnetic nanoparticles, belonging to the technical field of carbon-based composite materials; the method is to obtain an intermediate 1 graphite phase carbon nitride g-C3N4 powder by placing melamine C3N6H6 in a tube furnace under air conditions and calcining at high temperature; then disperse it in an ethanol solvent with an iron metal salt, wherein the mass ratio of the intermediate 1 to the iron metal salt is 1:1~3, and obtain an intermediate 2 by ultrasound, magnetic stirring, and drying; finally, the intermediate 2 is calcined at high temperature under the protection of inert gas argon, and finally a carbon microsphere-loaded magnetic nanoparticle composite wave absorbing material is obtained. The present invention utilizes a simple two-step high-temperature calcination to prepare a carbon microsphere-loaded magnetic nanoparticle composite wave absorbing material, and the final product has excellent electromagnetic wave absorption capacity, and the preparation method is simple to operate, and the electromagnetic parameters of the product are controllable and adjustable, thereby regulating the electromagnetic wave absorption capacity of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon-based composite materials, and in particular relates to a method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles. Background Art

[0002] With the rapid development of high-tech and cutting-edge technologies, a large number of electronic equipment and communication facilities have become popular in the civil and military fields. However, while providing convenience for human life, it also causes serious electromagnetic interference and electromagnetic pollution problems, and puts forward higher requirements for microwave absorbing materials. Designing and synthesizing new absorbing materials with excellent microwave absorption performance is the most important and effective technical and tactical means, which can absorb and attenuate adverse electromagnetic waves through energy conversion, thereby preventing electromagnetic pollution and improving the survivability, penetration and deep strike capabilities of weapon systems.

[0003] Carbon materials have good application prospects in the field of electromagnetic wave absorption due to their low density, high oxidation resistance, significant dielectric properties and excellent mechanical properties, including graphene, carbon nanotubes, porous carbon, carbon fiber, etc. However, carbon materials generally have high electrical conductivity, which causes electromagnetic waves to be reflected more on their surface rather than entering the interior of the material for attenuation, which is not conducive to absorption. Compounding them with magnetic loss materials through certain technical means can not only solve the problem of high density and poor dispersion of magnetic nanoparticles, but also effectively enhance the electromagnetic wave absorption performance, broaden the absorption frequency band, and achieve high-intensity, light-weight, and broadband absorption effects.

[0004] In addition, in order to obtain an ideal absorber material, reasonable microstructure design also plays an important role in the absorption performance. For example, the published paper "Carbon hollow microspheres with a designable mesoporous shell for high-performance electromagnetic wave absorption" describes a method for preparing hollow carbon microspheres, which is to first use a hard template method and a pyrolysis etching process to prepare hollow carbon microspheres. However, the preparation process is complicated, and highly corrosive and hydrofluoric acid are used. In addition, due to the lack of magnetic components in its composition, its matching performance is poor, and the absorption performance cannot meet the requirements.

[0005] Therefore, there is an urgent need to design a carbon-based composite absorbing material loaded with magnetic nanoparticles, which has excellent matching performance and significantly improved absorbing performance. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of complex preparation process and poor absorption performance of composite absorbing materials in the prior art, and to provide a method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles. The carbon microsphere composite material containing magnetic nanoparticles is prepared through a simple mechanical mixing and high-temperature calcination process. The obtained magnetic carbon microspheres have a wider effective absorption band and a stronger reflection loss value, and have excellent absorption performance.

[0007] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, comprising the following steps:

[0008] S1, graphite carbon nitride gC 3 N 4 Preparation: Melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 400~700℃ to prepare graphite carbon nitride gC 3 N 4 , as intermediate 1;

[0009] S2, gC 3 N 4 @Preparation of metal salt: dissolve iron metal salt in ethanol to prepare a solution, and add the intermediate 1 prepared in the above step S1 to obtain a mixed solution, wherein the mass ratio of the intermediate 1 to the iron metal salt is 1:1-3, and dry the mixed solution after ultrasonic and magnetic stirring to obtain a mixed powder loaded with metal salt as intermediate 2;

[0010] S3, Carbon microspheres C@Fe 3 O 4 Preparation: The intermediate 2 powder prepared in the above step S2 is placed in a tube furnace and calcined at a high temperature in an inert atmosphere of argon at a temperature of 500-900°C for a time of 1-3 hours to obtain a carbon microsphere-loaded magnetic nanoparticle composite.

[0011] In the step S1, preferably, the calcination temperature is 500°C.

[0012] In the step S1, the calcination time is 1 to 5 hours, preferably, the calcination time is 3 hours.

[0013] In the step S2, preferably, the mass ratio of the intermediate 1 to the iron metal salt is 1:1.

[0014] In step S2, the iron metal salt includes one or more of ferric nitrate, ferric acetate, and ferric chloride.

[0015] In the step S3, preferably, the calcination temperature is 750° C. and the calcination time is 2 h.

[0016] The beneficial effects of the present invention are:

[0017] 1) The present invention has successfully prepared a composite material of carbon microspheres loaded with magnetic nanoparticles through X-ray diffraction, Raman spectroscopy and scanning electron microscopy, and the structure is consistent with expectations. The electromagnetic parameters are tested using a network vector analyzer (VNA), and the wave absorption performance is simulated and calculated using Matlab software. The data results show that the composite material of carbon microspheres loaded with magnetic nanoparticles has excellent electromagnetic wave absorption performance, good impedance matching performance and electromagnetic wave attenuation performance, and achieves the purpose of fully absorbing and attenuating electromagnetic waves.

[0018] 2) Compared with the existing methods, the present invention has the advantages of simple preparation method, green and safe, and the obtained magnetic carbon microspheres have a wider effective absorption band and a stronger reflection loss value, and have excellent wave absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 C@Fe prepared in Example 1 of the present invention 3 O 4 SEM images of microsphere composites;

[0020] Figure 2 C@Fe prepared in Example 1 of the present invention 3 O 4 Raman spectra of microsphere composites;

[0021] Figure 3 C@Fe prepared in Example 1 of the present invention 3 O 4 X-ray diffraction spectrum of microsphere composites;

[0022] Figure 4 C@Fe prepared in Example 1 of the present invention 3 O 4 Reflection loss curve of microsphere composite material;

[0023] Figure 5 C@Fe prepared in Examples 1 to 5 of the present invention 3 O 4 Reflection loss curve of microsphere composite material at the same thickness d=2.4mm;

[0024] Figure 6 C@Fe prepared in control group 1 of the present invention 3 O 4 Reflection loss curve of microsphere composite material;

[0025] Figure 7 C@Fe prepared in control group 2 of the present invention 3 O4 Reflection loss curve of microsphere composite material;

[0026] Figure 8 C@Fe prepared in control group 3 of the present invention 3 O 4 Reflection loss curve of microsphere composite material. DETAILED DESCRIPTION

[0027] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.

[0028] Example 1: A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, comprising the following steps:

[0029] S1, graphite carbon nitride gC 3 N 4 Preparation of -1: 4g melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 500°C for 3 hours to prepare graphite carbon nitride gC 3 N 4 -1;

[0030] S2, gC 3 N 4 @ Preparation of metal salt-1: 1 g of the graphite phase carbon nitride gC 3 N 4 -1, added to 1g FeCl 3 40mL ethanol solution (with crystal water) was added, ultrasonically stirred for 30 minutes, and then the mixed solution was dried to obtain a powder, which was gC 3 N 4 @Metal salt-1;

[0031] S3, Carbon microspheres C@Fe 3 O 4 Preparation of -1: The gC 3 N 4 The metal salt-1 powder was placed in a tube furnace and calcined at 750°C in an inert atmosphere of argon for 2 hours to obtain carbon microspheres loaded with magnetic Fe 3 O 4 Composite Absorbing Particles C@Fe 3 O 4 -1.

[0032] Example 2: A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, comprising the following steps:

[0033] S1, graphite carbon nitride gC 3 N 4 Preparation of -2: 4 g of melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 400°C for 5 hours to prepare graphite carbon nitride gC 3 N 4 -2;

[0034] S2, gC 3 N 4 @ Preparation of metal salt-2: 1 g of the graphite phase carbon nitride gC 3 N 4 -2, added to a solution of 2g FeCl 3 40mL ethanol solution (with crystal water) was added, ultrasonically stirred for 30 minutes, and then the mixed solution was dried to obtain a powder, which was gC 3 N 4 @Metal salt-2;

[0035] S3, Carbon microspheres C@Fe 3 O 4 Preparation of -2: The gC 3 N 4 @Metal salt-2 powder was placed in a tube furnace and calcined in an inert atmosphere of argon at a high temperature of 500°C for 3 hours to obtain carbon microspheres loaded with magnetic Fe 3 O 4 Composite Absorbing Particles C@Fe 3 O 4 -2.

[0036] Embodiment 3: A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, comprising the following steps:

[0037] S1, graphite carbon nitride gC 3 N 4 Preparation of -3: 4 g melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 600°C for 3 hours to prepare graphite carbon nitride gC 3 N 4 -3;

[0038] S2, gC 3 N 4 @ Preparation of metal salt-3: 1 g of the graphite phase carbon nitride gC 3 N 4-3, added to 3g FeCl 3 40mL ethanol solution (with crystal water) was added, ultrasonically stirred for 30 minutes, and then the mixed solution was dried to obtain a powder, which was gC 3 N 4 @Metal salt-3;

[0039] S3, Carbon microspheres C@Fe 3 O 4 Preparation of -3: The gC 3 N 4 @Metal salt-3 powder was placed in a tube furnace and calcined in an inert atmosphere of argon at a high temperature of 900°C for 1 h to obtain carbon microspheres loaded with magnetic Fe 3 O 4 Composite Absorbing Particles C@Fe 3 O 4 -3.

[0040] Example 4: A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, comprising the following steps:

[0041] S1, graphite carbon nitride gC 3 N 4 Preparation of -4: 4g melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 700°C for 1 hour to prepare graphite carbon nitride gC 3 N 4 -4;

[0042] S2, gC 3 N 4 @ Preparation of metal salt-4: 1 g of the graphite phase carbon nitride gC 3 N 4 -4, added to 2g FeCl 3 40mL ethanol solution (with crystal water) was added, ultrasonically stirred for 30 minutes, and then the mixed solution was dried to obtain a powder, which was gC 3 N 4 @Metal salt-4;

[0043] S3, Carbon microspheres C@Fe 3 O 4 Preparation of -4: The gC 3 N 4 @Metal salt-4 powder was placed in a tube furnace and calcined in an inert atmosphere of argon at a high temperature of 500°C for 3 hours to obtain carbon microspheres loaded with magnetic Fe 3O 4 Composite Absorbing Particles C@Fe 3 O 4 -4.

[0044] Example 5: A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, comprising the following steps:

[0045] S1, graphite carbon nitride gC 3 N 4 Preparation of -5: 4 g melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 600°C for 3 hours to prepare graphite carbon nitride gC 3 N 4 -5;

[0046] S2, gC 3 N 4 @ Preparation of metal salt-5: 1 g of the graphite phase carbon nitride gC 3 N 4 -5, added to 1g FeCl 3 40mL ethanol solution (with crystal water) was added, ultrasonically stirred for 30 minutes, and then the mixed solution was dried to obtain a powder, which was gC 3 N 4 @Metal salt-5;

[0047] S3, Carbon microspheres C@Fe 3 O 4 Preparation of -5: The gC 3 N 4 The metal salt-5 powder was placed in a tube furnace and calcined at 750°C in an inert atmosphere of argon for 3 hours to obtain carbon microspheres loaded with magnetic Fe 3 O 4 Composite Absorbing Particles C@Fe 3 O 4 -5.

[0048] Control group 1: except that the calcination temperature in step S1 is 800° C., the rest of the preparation process is the same as that of specific embodiment 1.

[0049] Control group 2: except for the graphite phase carbon nitride gC in step S2 3 N 4 Except that the mass ratio of the metal salt is 1:4, the rest of the preparation process is the same as that of Specific Example 2.

[0050] Control group 3: except that the calcination temperature in step S3 is 400° C., the rest of the preparation process is the same as that of specific embodiment 3.

[0051] The test results of the performance of the prepared materials in the above examples are as follows:

[0052] Figure 1 C@Fe 3 O 4 -1Scanning electron microscope image of the composite material. It can be seen from the figure that C@Fe 3 O 4 -1 composite material exhibits a distinct spherical morphology.

[0053] Figure 2 C@Fe 3 O 4 -1 Raman spectrum of composite absorbing material. It can be seen from the figure that C@Fe 3 O 4 -1 composite absorbing material has obvious D peak and G peak, indicating that the final product contains graphite carbon.

[0054] Figure 3 C@Fe 3 O 4 -1 X-ray diffraction spectrum of composite absorbing material, the peak position is similar to that of Fe 3 O 4 The standard PDF card is consistent with that of the standard PDF card, and a broad carbon diffraction peak appears near 26.00, indicating the presence of graphite carbon, indicating that the composition of the final product is graphite carbon and Fe 3 O 4 .

[0055] Figure 4 C@Fe 3 O 4 -1 Reflection loss curve of composite absorbing material. It can be seen from the figure that C@Fe 3 O 4 The -1 composite material has the minimum reflection loss value at a thickness of 3.9 mm.

[0056] Figure 5 C@Fe prepared in Examples 1 to 5 of the present invention 3 O 4 The reflection loss curve of the composite material at the same thickness of d=2.4mm shows that the absorption performance of the magnetic carbon microspheres at the same thickness obtained under different preparation conditions within the calcination temperature and mass ratio range is different, so the present invention can achieve controllable and adjustable performance.

[0057] Figure 6 , Figure 7 and Figure 8 C@Fe prepared for control groups 1 to 3 of the present invention 3O 4 The microwave absorption performance of the composite material shows that the calcination temperatures in control groups 1 and 3 and the mass ratio in control group 2 are both outside the range of Examples 1-5. Figures 6-8 It can be seen from the reflection loss values ​​in that its minimum reflection loss value is greater than the maximum reflection loss value of Example 1-5, and its wave absorbing performance is poor.

[0058] In addition, because the electromagnetic absorption performance is closely related to the electromagnetic parameters, similar effects can be achieved outside the data parameters of the present invention by adjusting the calcination temperature, the ratio of raw materials and the filling ratio with the paraffin matrix under relative conditions.

[0059] The method of the present invention utilizes a simple two-step high-temperature calcination to prepare a carbon microsphere-loaded magnetic nanoparticle composite absorbing material. The final product has excellent electromagnetic wave absorption capacity, and the preparation method is simple to operate. At the same time, the electromagnetic parameters of the product are controllable and adjustable to thereby regulate the electromagnetic wave absorption capacity of the composite material; and the product has good impedance matching performance and electromagnetic wave attenuation performance, thereby achieving the purpose of fully absorbing and attenuating electromagnetic waves.

[0060] The above description is only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in this field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles, Features: The following steps are involved: S1, graphite carbon nitride gC 3 N 4 Preparation: Melamine C 3 N 6 H 6 Place it in a tube furnace and calcine it in air at a high temperature of 400~700℃ to prepare graphite carbon nitride gC 3 N 4 , as intermediate 1; S2, gC 3 N 4 @Preparation of metal salt: dissolve iron metal salt in ethanol to prepare a solution, and add the intermediate 1 prepared in the above step S1 to obtain a mixed solution, wherein the mass ratio of the intermediate 1 to the iron metal salt is 1:1-3, and dry the mixed solution after ultrasonic and magnetic stirring to obtain a mixed powder loaded with metal salt as intermediate 2; The iron metal salt includes one or more of ferric nitrate, ferric acetate and ferric chloride; S3, Carbon microspheres C@Fe 3 O 4 Preparation: The intermediate 2 powder prepared in the above step S2 is placed in a tube furnace and calcined at a high temperature in an inert atmosphere of argon at a temperature of 500-900°C for a time of 1-3 hours to obtain a carbon microsphere-loaded magnetic nanoparticle composite.

2. The method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles according to claim 1, Features: In the step S1, the calcination temperature is 500°C.

3. The method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles according to claim 1, Features: In the step S1, the calcination time is 1 to 5 hours.

4. The method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles according to claim 3, Features: In the step S1, the calcination time is 3 hours.

5. The method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles according to claim 1, Features: In the step S2, the mass ratio of the intermediate 1 to the iron metal salt is 1:

1.

6. The method for preparing a composite material of carbon microspheres loaded with magnetic nanoparticles according to claim 1, Features: In step S3, the calcination temperature is 750° C. and the calcination time is 2 h.