A fixed bed hydrogenation reactor and a method for producing reforming raw materials

By partitioning and combining catalysts in the hydrogenation reactor, the treatment problems of sulfur, nitrogen and cyclosiloxane in coking naphtha are solved, the device operation cycle is extended and energy consumption is reduced, and the efficient reforming raw materials are achieved Production.

CN116037002BActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111260971.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-11-08
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

In the prior art, it is difficult to effectively reduce the sulfur, nitrogen content in coking naphtha and the problem of carbon accumulation and silicone blockage caused by cyclosiloxane in the catalyst bed during the hydrorefining process. In addition, when inferior naphtha is used as a reforming raw material, it is added. The hydrogen device has a harsh reaction scale and high energy consumption.

Method used

A fixed-bed hydrogenation reactor was designed, and the first, second and third hydrogenation zones were set up by partitioning the hydrogenation zones, and the combination of different catalysts and silicon trapping agents was used to optimize the process flow to reduce the temperature of the catalyst bed and separate the and treat high olefin, high sulfur and high nitrogen fractions, combine appropriate catalyst and silicon trapping agent ratios, control the reaction temperature and hydrogen partial pressure, and extend the operation cycle of the device.

Benefits of technology

It effectively reduces the temperature of the catalyst bed, extends the operation cycle of the device, improves the quality of reforming raw materials, reduces hydrogen and energy consumption, and avoids rapid catalyst deactivation and carbon deposit problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116037002B_ABST
    Figure CN116037002B_ABST
Patent Text Reader

Abstract

The present invention discloses a fixed-bed hydrogenation reactor and a method for producing reforming raw materials. The fixed-bed hydrogenation reactor is provided with a hydrogenation zone 1, a flash zone, a hydrogenation zone 2 and a hydrogenation zone 3 from top to bottom. The method for producing reforming raw materials comprises: the raw materials enter from the flash zone, and after flashing, a gas phase fraction and a liquid phase fraction are obtained, the gas phase fraction enters the hydrogenation zone 1 and undergoes a hydrogenation reaction, the gas phase reaction product is discharged from the top of the reactor, condensed and circulated back to the hydrogenation zone 2, and mixed with the liquid phase fraction obtained by flashing, silicon capture and deolefination, desulfurization, and denitrogenation reactions occur; the effluent from the hydrogenation zone 2 flows downward and is further mixed and dissolved with the hydrogen entering, and enters the hydrogenation zone 3 for a liquid phase hydrogenation reaction, and the hydrogenation reaction product flows out from the bottom as a reforming raw material. This method uses inferior and heavy naphtha as raw materials, and by optimizing the process flow and matching a suitable catalyst, it can meet the requirements of the catalytic reforming process for raw materials and extend the operation cycle of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil refining and chemical industry, and specifically relates to a fixed bed hydrogenation reactor and a method for producing reforming raw materials. Background Art

[0002] After further hydrogenation and refining, the naphtha fraction can be used as ethylene raw material, synthetic ammonia raw material and catalytic reforming raw material, etc. It can also be used as a blending component for motor gasoline. In recent years, as my country's oil refining industry continues to transform towards the chemical industry, the production demand for aromatics has increased significantly year by year. Aromatics are an important basic raw material for organic chemical industry. Aromatics obtained by reforming can be used as solvents, produce polyester fibers, manufacture plasticizers, and be used in the production of pesticides, dyes, and medicines after further conversion, separation and purification. Therefore, continuously optimizing naphtha hydrogenation technology to support the raw material demand of my country's chemical industry is one of the current focuses of technology research and development in the oil refining field.

[0003] At present, the reforming raw material is mainly straight-run naphtha, which has relatively low impurities such as sulfur and nitrogen, high paraffin content and high aromatic potential. It can be used as a high-quality reforming raw material after simple hydrogenation refining. However, due to the current large domestic ethylene gap, some straight-run naphtha must be used as ethylene raw materials, which will compete with reforming raw materials. Therefore, further expanding the source of reforming raw materials and using heavier and inferior naphtha fractions as reforming raw materials is one of the current hot spots in technology research and development, including coking naphtha, heavy-cut high-nitrogen straight-run naphtha, catalytic cracking gasoline, catalytic cracking gasoline, etc.

[0004] Coking naphtha is one of the products of delayed coking unit. It not only has relatively high sulfur and nitrogen content, but also has high olefin content (about 40%) because it is a product of thermal cracking reaction. At the same time, since delayed coking unit often adds silicon-containing defoaming agent to suppress foaming, cyclosiloxane is formed in the delayed coking unit, and its boiling point is about 150℃. Therefore, it will follow into the naphtha fraction after coking, resulting in 10~20ppm Si in the coking naphtha. At present, industrial coking naphtha hydrogenation unit generally adopts two reactors in series. The pre-protection reactor removes dienes at a low temperature of about 120℃, and then removes monoolefins, Si and impurities such as S and N in the main reactor. The main inlet temperature of the main reactor is generally 220℃ and 360℃. The following problems are often encountered during operation: 1. After the dienes are removed at low temperature in the pre-protection reactor, the coking naphtha still contains a large amount of monoolefins. The olefins release a lot of heat during the hydrogenation reaction in the main reactor, causing the catalyst bed temperature to rise rapidly, causing carbon deposits to form on the catalyst surface. If there is a trace amount of oxygen in the raw material, the olefin coking and carbon deposition will be more serious. At this time, the catalyst can only be active at a higher temperature. The vicious cycle causes the catalyst to deactivate quickly and the bed pressure drop is forced to stop. 2. The cyclosiloxane contained in the coking naphtha is a large molecular species. When the catalyst bed temperature is high, the cyclosiloxane will react with hydrogen to generate silica gel to block the catalyst pores. At present, industrial devices generally adopt the method of filling the first bed of the reactor with silicon scavengers. Under the condition of relatively low reaction temperature in the upper part of the reactor, the large molecular silicon-containing compounds are converted into small molecules and then adsorbed and removed.

[0005] In order to reduce the diesel fraction and increase the production of gasoline and chemical products, oil refineries currently generally cut heavy naphtha fractions, which will lead to a significant increase in the sulfur and nitrogen content in naphtha raw materials. Catalytic cracking and catalytic cracking gasoline also have problems with high olefin, sulfur and nitrogen content. Since the sulfur and nitrogen content of reforming feed is very strictly restricted, requiring less than 0.5μg / g, this puts forward higher hydrogenation depth requirements for blending inferior and heavy naphtha as reforming feed, and requires increasing the reaction severity of the hydrogenation unit, increasing hydrogen consumption and energy consumption.

[0006] CN109420513A discloses a catalyst for pretreatment of inferior reforming raw materials and a preparation method thereof, which can reduce sulfur and nitrogen in coking naphtha raw materials to below 0.5 μg / g, and the generated oil after hydrogenation meets the feed requirements of the reforming device. However, the catalyst fails to solve the restriction requirements of Si content in the raw materials, and due to the high inlet temperature of the reactor, it is also impossible to avoid the influence of coking and carbon deposition caused by the large amount of heat release of olefin hydrogenation reaction in coking naphtha on its life. This catalyst is also not well suited for deep refining of high-nitrogen raw materials. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention proposes a fixed bed hydrogenation reactor and a method for producing reforming raw materials. The method uses inferior and heavy naphtha as raw materials. By optimizing the process flow and matching a suitable catalyst, the requirements of the catalytic reforming process for raw materials can be met and the operation cycle of the device can be extended.

[0008] The fixed bed hydrogenation reactor of the present invention is provided with a first hydrogenation zone, a flash zone, a second hydrogenation zone and a third hydrogenation zone in sequence from top to bottom; a liquid phase material inlet is provided in the flash zone, and a hydrogen inlet is provided between the second hydrogenation zone and the third hydrogenation zone;

[0009] The hydrogenation zone 1 is a gas phase hydrogenation reaction zone, which is used for deolefination, desulfurization and denitrogenation reactions of gas phase fractions below 140-150°C; the first hydrogenation catalyst is loaded in the hydrogenation zone 1; a gas phase outlet is arranged at the top of the hydrogenation zone 1, the gas phase outlet is connected to a condensation device via a pipeline, and the condensation device is connected to the top of the hydrogenation zone 2 via a pipeline; the hydrogenation product of the gas phase fraction is condensed and circulated back to the hydrogenation zone 2;

[0010] The flash evaporation zone is used to flash the liquid raw material into a gas phase fraction and a liquid phase fraction, wherein the gas phase fraction (the fraction below 140-150°C) enters the first hydrogenation zone, and the liquid phase fraction (the fraction above 150°C) enters the second hydrogenation zone;

[0011] The second hydrogenation zone is a gas-liquid hydrogenation reaction zone, which is used for the liquid phase fraction after flash evaporation and the liquid phase product recycled from the first hydrogenation zone after heat exchange to undergo deolefination, desulfurization, denitrification and silicon capture reactions; the second hydrogenation catalyst and silicon capture agent are graded and loaded in the second hydrogenation zone;

[0012] The hydrogenation zone 3 is a liquid phase hydrogenation reaction zone, which is used for deep denitrification reaction of the reaction effluent of the hydrogenation zone 2; the second hydrogenation catalyst is loaded in the hydrogenation zone 3; a material outlet is set at the bottom of the hydrogenation zone 3; and a high-efficiency hydrogen mixer assembly is preferably set at the top of the hydrogenation zone 3.

[0013] The present invention also provides a method for producing reforming raw materials, which comprises the following contents: hydrogen enters between the second hydrogenation zone and the third hydrogenation zone of a fixed bed reactor; inferior naphtha raw materials enter from the flash distillation zone, and after flash distillation, an upward-flowing gas phase fraction and a downward-flowing liquid phase fraction are obtained, the gas phase fraction enters the first hydrogenation zone to undergo a hydrogenation reaction with a first hydrogenation catalyst, a gas phase reaction product is discharged from the top of the reactor, condensed and circulated back to the second hydrogenation zone, mixed with a liquid phase fraction obtained by flash distillation, and passed through a graded silicon trapping agent and a second hydrogenation catalyst to undergo silicon trapping and olefin removal, desulfurization and denitrogenation reactions; the effluent from the second hydrogenation zone flows downward to be further mixed and dissolved with the entering hydrogen, enters the third hydrogenation zone to undergo a liquid phase hydrogenation reaction with a third hydrogenation catalyst, and the hydrogenation reaction product flows out from the bottom of the reactor as a reforming raw material.

[0014] In the production method of the present invention, the inferior naphtha raw material is coker naphtha or coker naphtha blended with other inferior raw materials, and the inferior raw materials are one or more of cut-weight straight-run naphtha, catalytic cracking gasoline, and catalytic cracking naphtha (hereinafter referred to as DCC naphtha), with no restriction on the blending ratio; the distillation range is 30-220°C, S≯10000μg / g, N≯500μg / g, and olefins≯50%.

[0015] In the production method of the present invention, the flash zone is used to separate the fraction below 140-150°C from the inferior naphtha raw material and enter the hydrogenation zone 1 in the gas phase, and the fraction above 150°C enters the hydrogenation zone 2 in the liquid phase; the operating conditions of the flash zone are: pressure 1.0-6.0MPa, preferably 2.0-4.0MPa, wherein the hydrogen partial pressure accounts for 45%-80% of the total pressure; the feed temperature is 100-200°C, preferably 130-180°C; the hydrogen-to-oil volume ratio is 10:1-800:1, preferably 100:1-400:1.

[0016] In the production method of the present invention, the operating conditions of the first hydrogenation zone are: pressure 1.0~8.0MPa, preferably 2.0~6.0MPa, wherein the hydrogen partial pressure accounts for 40%~70% of the total pressure; volume space velocity 0.1~10.0h -1 , preferably 0.5~6.0h -1 ; Reaction temperature is 50-180°C, preferably 80-150°C; hydrogen-to-oil volume ratio is 10:1-400:1, preferably 100:1-200:1. The first hydrogenation catalyst comprises a VIB group metal sulfide, a VIII group metal oxide and an alumina carrier; based on the total weight of the catalyst, the content of the VIB group metal sulfide is 5wt%-30wt%, preferably 15-25%, the content of the VIII group metal oxide is 3wt%-15wt%, preferably 3-8%, and the balance is an alumina carrier; wherein the VIB group metal is selected from at least one of Mo and W, and the VIII group metal is selected from at least one of Co and Ni; wherein the hydrogenation catalyst (oxidation state) is analyzed by XPS spectrum, and the molar ratio of the +4 valence VIB group metal to the total amount of the VIB group metal is 60%-90%.

[0017] In the production method of the present invention, the second hydrogenation zone is used for the liquid phase fraction after flash evaporation and the liquid phase product recycled from the first hydrogenation zone to undergo deolefination, desulfurization and denitrogenation reactions. The filling volume ratio of the silicon scavenger to the first hydrogenation catalyst in the second hydrogenation zone is 6:1~1:6, which is adjusted according to the actual silicon content in the raw materials. The silicon scavenger is a commonly used commercial silicon scavenger, such as the FHRS series silicon scavengers developed by FRIPP.

[0018] In the production method of the present invention, the operating conditions of the second hydrogenation zone are generally: pressure 1.0~8.0MPa, preferably 2.0~6.0MPa, wherein the hydrogen partial pressure accounts for 40%~70% of the total pressure; volume space velocity 0.1~10.0h -1 , preferably 0.5~6.0h -1 ; Reaction temperature 80~180℃, preferably 100~150℃; Hydrogen to oil volume ratio 10:1~400:1, preferably 100:1~200:1.

[0019] The preparation method of the first hydrogenation catalyst comprises the following contents:

[0020] (1) impregnating a hydrogenation catalyst support with an impregnation solution containing a Group VIB metal, followed by drying and sulfiding;

[0021] (2) The catalyst sulfided in step (1) is impregnated with an impregnation solution containing a Group VIII metal, and then dried and calcined in an inert atmosphere to obtain a hydrogenation catalyst.

[0022] The preparation method of the impregnation solution of the VIB group metal in step (1) is well known to those skilled in the art, such as generally using a phosphate or ammonium salt solution, the mass concentration of the impregnation solution is 0.1 g / mL to 2.4 g / mL, and an equal volume impregnation method can be used. The VIB group metal is preferably Mo and / or W.

[0023] The drying conditions in step (1) are: drying temperature 100-220° C., and drying time 2-6 hours.

[0024] The vulcanization treatment in step (1) is well known to those skilled in the art, and is usually carried out by dry vulcanization or wet vulcanization. The dry vulcanizing agent is hydrogen sulfide, and the wet vulcanizing agent is carbon disulfide, dimethyl disulfide, etc.; the vulcanization pressure is 3.5-6.5 MPa, the vulcanization temperature is 220-380°C, and the vulcanization time is 3-10 h.

[0025] The preparation method of the impregnation solution of the Group VIII metal in step (2) is well known to those skilled in the art. For example, acetate, nitrate, sulfate and other solutions are generally used. The mass concentration of the impregnation solution is 0.14 g / mL~1.4 g / mL. An equal volume impregnation method can be adopted. The Group VIII metal is Ni and / or Co.

[0026] The inert atmosphere in step (2) is one or more inert gases; the drying temperature is 40-120°C, and the drying time is 2-12 hours; the roasting temperature is 240-550°C, and the roasting time is 3-8 hours.

[0027] In the production method of the present invention, the third hydrogenation catalyst loaded in the hydrogenation zone is a hydrodenitrogenation catalyst, such as the FH-40 or FHUDS series hydrogenation catalyst developed by FRIPP. The operating conditions of the hydrogenation zone are: pressure 1.0~10.0MPa, preferably 3.0~8.0MPa; volume space velocity 0.1~8.0h -1 , preferably 0.5~6.0h -1 ; The reaction temperature is 80~220℃, preferably 120~200℃.

[0028] The present invention effectively controls the problem of excessive temperature rise of the catalyst bed of the inferior naphtha hydrogenation unit, and realizes the production of reforming raw materials under mild conditions in one reactor. The inferior naphtha raw material is firstly divided into two gas and liquid components by flash evaporation, and the raw materials with high olefin, high sulfur and high nitrogen content are divided into two regions for reaction. The components refined by hydrogenation in the first hydrogenation zone are condensed and circulated to the second hydrogenation zone, which can dilute the olefin concentration of the components in the second hydrogenation zone and weaken the heat release of the olefin reaction. At the same time, the condensed components can also reduce the bed temperature, which plays a role in controlling the temperature rise of the bed in the second hydrogenation zone. Combined with the use of the first hydrogenation catalyst, the catalyst is a partially sulfurized hydrogenation catalyst, which does not need to be sulfurized before use. As the reaction proceeds, the hydrogen sulfide in the system is gradually sulfurized, and the low-temperature activity is good and the initial activity is stable. The reaction inlet feed temperature (150°C flash evaporation) is greatly reduced compared with the conventional technology (about 220°C at the inlet), and the liquid phase material descending after gas-liquid separation can also be kept in the liquid phase state to react, and the concentrated and violent heat release of olefins due to excessive initial activity will not make the catalyst bed temperature difficult to control. At the same time, the flash separation temperature at the raw material inlet is controlled below 150°C. Since the boiling point of the silicon-containing species in the raw material - cyclosiloxane is above 150°C, Si will not enter the first hydrogenation zone with the gas phase. There is no need to load silicon scavengers in the first hydrogenation zone, and Si can be removed centrally in the second hydrogenation zone.

[0029] Since the sulfur and olefin content in the materials entering the third hydrogenation zone has been significantly reduced, the deep denitrification reaction mainly occurs in this reaction zone. Since the hydrogen enters between the second and third hydrogenation zones, the hydrogen partial pressure in the third hydrogenation zone can be guaranteed to be relatively high, which is conducive to the occurrence of deep hydrogenation reactions. At the same time, the upward hydrogen will take away the generated gas phase light hydrocarbons in time, and the liquid phase entering the third hydrogenation zone contains almost no low molecular weight hydrocarbons and hydrogen sulfide, which is conducive to increasing the solubility of hydrogen in the liquid phase and further promoting the hydrogenation reaction. The upward hydrogen plays a role in balancing the temperature distribution in the entire reactor and stripping hydrogen sulfide. It can not only avoid the accumulation of hydrogen sulfide in the reactor, but also carry hydrogen sulfide to the surface of the semi-sulfurized catalyst loaded in the first and second reaction zones, gradually activating the catalyst and ensuring long-term operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic flow diagram of the method for producing reforming raw materials of the present invention.

[0031] In the figure: 1- low-quality naphtha feedstock, 2- hydrogen, 3- hydrogenation zone 1, 4- hydrogenation zone 2, 5- hydrogenation zone 3, 6- flash zone, 7- gas phase reaction product, 8- condenser, 9- refined naphtha product. DETAILED DESCRIPTION

[0032] The present invention will be described in detail below with reference to the accompanying drawings and embodiments, but the present invention is not limited thereto.

[0033] Attach Figure 1 Take the example to illustrate the implementation process of the reforming raw material production method of the present invention: inferior naphtha raw material 1 enters the flash zone 6 under certain temperature and pressure conditions, and the gas and liquid are separated into gas phase and liquid phase in the flash zone 6. The gas phase flows upward into the hydrogenation zone 1 3, and the liquid phase flows downward into the hydrogenation zone 2 4. Hydrogen 2 enters the fixed bed reactor between the hydrogenation zone 2 4 and the hydrogenation zone 3 5, and after mixing and contacting with the liquid phase material flowing downward from the hydrogenation zone 2 4, the excess hydrogen continues to flow upward into the hydrogenation zone 2 4, and the liquid phase material dissolved and carrying hydrogen flows downward into the hydrogenation zone 3 5; a gas phase reaction occurs in the hydrogenation zone 1 3, mainly the hydrodesulfurization, denitrogenation, and olefin saturation reaction of the fraction below 150°C in the raw material, to generate a gas phase product 7 which is condensed by the condenser 8 and circulated to the hydrogenation zone 2 4. A gas-liquid two-phase reaction occurs in the hydrogenation zone 2 4, wherein the liquid phase is the fraction above 150°C in the feedstock flowing downward, and the gas phase is the hydrogen flowing upward, and the gas and liquid are in reverse contact to cause desiliconization, desulfurization, denitrogenation and olefin saturation reactions; the hydrogen sulfide and low molecular weight hydrocarbons generated by the reaction flow upward with the gas phase flow into the hydrogenation zone 2 4 and the hydrogenation zone 1 3, and finally flow out from the top of the hydrogenation zone 1 (reactor); the liquid phase flow after hydrogenation flows downward into the hydrogenation zone 3 5, and the hydrogenation zone 3 5 is a liquid phase reaction, and the liquid phase components react with the dissolved hydrogen to undergo a deep denitrogenation reaction to generate a refined naphtha product 9.

[0034] Example 1

[0035] Ammonium heptamolybdate was adjusted with ammonia water until it was completely dissolved, and an impregnation solution with a concentration of 0.16 g / mL was prepared, and then impregnated into the alumina support by an equal volume impregnation method, and dried at 150°C for 4 hours. Then DMDS was used for sulfurization treatment, the sulfurization pressure was 4.6 MPa, the sulfurization temperature was 330°C, the sulfurization time was 5 hours, and then cooled to room temperature in a N2 atmosphere to obtain MoS2 / Al2O3.

[0036] Cobalt nitrate was dissolved in deionized water to prepare an impregnation solution with a concentration of 0.15 g / mL, and the solution was impregnated onto MoS2 / Al2O3 using an equal volume impregnation method. The solution was then dried at 80°C for 3 h in a N2 atmosphere and calcined at 300°C for 3 h to obtain MoS2-CoO / Al2O3 catalyst C1.

[0037] Example 2

[0038] Ammonium heptamolybdate was adjusted with ammonia water until it was completely dissolved, and an impregnation solution with a concentration of 0.18 g / mL was prepared, and then impregnated into the alumina support by an equal volume impregnation method, and dried at 160°C for 4 hours. Then, hydrogen containing 3.0% H2S was used for sulfidation treatment, the sulfidation temperature was 350°C, the sulfidation pressure was 5.0 MPa, the sulfidation time was 4 hours, and then it was cooled to room temperature in a N2 atmosphere to obtain MoS2 / Al2O3.

[0039] Nickel nitrate was dissolved in deionized water to prepare an impregnation solution with a concentration of 0.15 g / mL, and the solution was impregnated onto MoS2 / Al2O3 using an equal volume impregnation method. The solution was then dried at 90°C for 3 h in a N2 atmosphere and calcined at 250°C for 3 h to obtain MoS2-NiO / Al2O3 catalyst C2.

[0040] Example 3

[0041] Ammonium metatungstate was adjusted with ammonia water until it was completely dissolved, and an impregnation solution with a concentration of 0.16 g / mL was prepared, and then impregnated into the alumina support by an equal volume impregnation method, and dried at 150°C for 4 hours. Then DMDS was used for sulfurization treatment, the sulfurization temperature was 360°C, the sulfurization pressure was 4.0 MPa, the sulfurization time was 5 hours, and then it was cooled to room temperature in a N2 atmosphere to obtain MoS2 / Al2O3.

[0042] Cobalt nitrate was dissolved in deionized water to prepare an impregnation solution with a concentration of 0.21 g / mL, and the solution was impregnated onto MoS2 / Al2O3 using an equal volume impregnation method. The solution was then dried at 100°C for 4 h in a N2 atmosphere and calcined at 280°C for 3 h to obtain MoS2-CoO / Al2O3 catalyst C3.

[0043] Comparative Example 1

[0044] Ammonium molybdate and cobalt nitrate were dissolved in deionized water, and then impregnated into an alumina support in equal volumes. The catalyst was dried at 130°C for 3 h and calcined at 350°C for 4 h to obtain MoO3-CoO / Al2O3 catalyst D1.

[0045] Embodiment 4-6

[0046] A catalyst bed is set in the hydrogenation zone 1, zone 2 and zone 3 of the fixed bed reaction. One of the semi-sulfurized catalysts C1-C3 is loaded in the hydrogenation zone 1, and a silicon scavenger and one of the hydrogenation catalysts C1-C3 are loaded in the hydrogenation zone 2. The silicon scavenger is the FHRS-2 silicon scavenger developed by FRIPP, and the volume ratio of the silicon scavenger to the hydrogenation catalyst is 2:1. The hydrogenation zone 3 is loaded with the FH-40D catalyst developed by FRIPP. A mixed oil of coking naphtha and high-nitrogen straight-run naphtha is used as the raw material, and the blending ratio is coking naphtha: high-nitrogen straight-run naphtha = 1:1. The properties of the catalyst are shown in Table 1, the properties of the raw oil are shown in Table 2, and the reaction process conditions and results are shown in Table 3.

[0047] Comparative Example 2

[0048] A catalyst bed is set in each of the hydrogenation zone 1, hydrogenation zone 2 and hydrogenation zone 3 of the fixed bed reaction. The D1 catalyst prepared in Comparative Example 1 is loaded in the hydrogenation zone 1, and the silicon trap and the D1 catalyst prepared in Comparative Example 1 are loaded in the hydrogenation zone 2, wherein the silicon trap and the catalyst and loading scheme of the hydrogenation zone 3 are the same as those of Examples 4-6. The same raw materials as those of Examples 4-6 are used, the properties of the catalyst are shown in Table 1, the properties of the feed oil are shown in Table 2, and the reaction process conditions and results are shown in Table 3.

[0049] Comparative Example 3

[0050] A conventional coking naphtha hydrogenation system was used, and the main reactor was equipped with three beds, the first bed was filled with FHRS-2 silicon trap developed by FRIPP, and the second and third beds were filled with conventional hydrorefining catalyst D1. The same raw materials as in Examples 4 to 6 were used, the catalyst properties are shown in Table 1, the raw oil properties are shown in Table 2, and the reaction process conditions and results are shown in Table 3.

[0051] Table 1 Physicochemical properties of catalysts

[0052]

[0053] Table 2 Raw oil properties

[0054]

[0055] Table 3 Hydrogenation process conditions and results

[0056]

[0057] Table 3 (Continued) Hydrogenation process conditions and results

[0058]

[0059] It can be seen from Table 3 that compared with the conventional fixed-bed hydrogenation process, this method can use coking naphtha and other inferior and heavy naphtha as raw materials to produce qualified reforming raw materials under milder operating conditions, which will be beneficial to the long-term stable operation of the device.

Claims

1. A fixed bed hydrogenation reactor, characterized in that: From top to bottom, hydrogenation zone 1, flash zone, hydrogenation zone 2 and hydrogenation zone 3 are arranged in sequence; a liquid material inlet is arranged in the flash zone, and a hydrogen inlet is arranged between hydrogenation zone 2 and hydrogenation zone 3; the flash zone is used to flash the liquid raw material into a gas phase fraction and a liquid phase fraction, the hydrogenation zone 1 is a gas phase hydrogenation reaction zone, which is used for deolefination, desulfurization and denitrogenation reactions of the gas phase fraction below 140-150°C; the hydrogenation zone 2 is a gas-liquid hydrogenation reaction zone, which is used for deolefination, desulfurization, denitrogenation and silicon capture reactions of the liquid phase fraction after flashing and the liquid phase product recycled from the hydrogenation zone 1 after heat exchange; the hydrogenation zone 3 is a liquid phase hydrogenation reaction zone, which is used for deep denitrification reaction of the reaction effluent of the hydrogenation zone 2.

2. The fixed bed hydrogenation reactor according to claim 1, characterized in that: The gas phase fraction obtained in the flash evaporation zone enters the first hydrogenation zone, and the liquid phase fraction enters the second hydrogenation zone.

3. The fixed bed hydrogenation reactor according to claim 1, characterized in that: The first hydrogenation catalyst is loaded in the first hydrogenation zone; a gas phase outlet is arranged at the top of the first hydrogenation zone, the gas phase outlet is connected to a condensation device via a pipeline, and the condensation device is connected to the top of the second hydrogenation zone via a pipeline; the gas phase fraction hydrogenation product is condensed and circulated back to the second hydrogenation zone.

4. The fixed bed hydrogenation reactor according to claim 1, characterized in that: The second hydrogenation zone is filled with a second hydrogenation catalyst and a silicon scavenger in a graded manner.

5. The fixed bed hydrogenation reactor according to claim 1, characterized in that: A material outlet is arranged at the bottom of the third hydrogenation zone; and a high-efficiency hydrogen mixer assembly is arranged at the top of the third hydrogenation zone.

6. A method for producing reforming raw materials, comprising the following contents: hydrogen enters between the second hydrogenation zone and the third hydrogenation zone of a fixed bed reactor; inferior naphtha raw material enters from the flash evaporation zone, and after flash evaporation, an upward-flowing gas fraction and a downward-flowing liquid fraction are obtained, the gas fraction enters the first hydrogenation zone for a hydrogenation reaction with a first hydrogenation catalyst, a gaseous reaction product is discharged from the top of the reactor, condensed and recycled back to the second hydrogenation zone, mixed with the liquid fraction obtained by flash evaporation, and passed through a graded silicon capture agent and a second hydrogenation catalyst to capture silicon and perform deolefination, desulfurization and denitrogenation reactions; the effluent from the second hydrogenation zone flows downward and is further mixed and dissolved with the entering hydrogen, enters the third hydrogenation zone for a liquid-phase hydrogenation reaction with a third hydrogenation catalyst, and the hydrogenation reaction product flows out from the bottom of the reactor as a reforming raw material.

7. The method according to claim 6, characterized in that: The inferior naphtha raw material is coker naphtha or coker naphtha mixed with other inferior raw materials, and the inferior raw materials are selected from one or more of cut-weight straight-run naphtha, catalytic cracking gasoline, and catalytic cracking naphtha; the distillation range is 30-220° C., S≯10000μg / g, N≯500μg / g, and olefins≯50%.

8. The method according to claim 6, characterized in that: The flash zone is used to separate the fraction below 140-150°C from the inferior naphtha raw material and enter the hydrogenation zone 1 in the gas phase, and the fraction above 150°C enters the hydrogenation zone 2 in the liquid phase; the operating conditions of the flash zone are: pressure 1.0-6.0MPa, wherein the hydrogen partial pressure accounts for 45%-80% of the total pressure; feed temperature 100-200°C, and hydrogen-to-oil volume ratio 10:1-800:

1.

9. The method according to claim 8, characterized in that: The operating conditions of the flash zone are: pressure 2.0~4.0MPa, feed temperature 130~180℃, hydrogen-to-oil volume ratio 100:1~400:

1.

10. The method according to claim 6, characterized in that: The operating conditions of the hydrogenation zone 1 are: pressure 1.0~8.0MPa, where the hydrogen partial pressure accounts for 40%~70% of the total pressure; volume space velocity 0.1~10.0h -1 , reaction temperature 50~180℃, hydrogen to oil volume ratio 10:1~400:

1.

11. The method according to claim 10, characterized in that: The operating conditions of the hydrogenation zone 1 are: pressure 2.0~6.0MPa, volume space velocity 0.5~6.0h -1 , reaction temperature 80~150℃, hydrogen-oil volume ratio 100:1~200:

1.

12. The method according to claim 6, characterized in that: The first hydrogenation catalyst comprises a VIB group metal sulfide, a VIII group metal oxide and an alumina carrier; based on the total weight of the catalyst, the content of the VIB group metal sulfide is 5wt%~30wt%, the content of the VIII group metal oxide is 3wt%~15wt%, and the balance is the alumina carrier; wherein the VIB group metal is selected from at least one of Mo and W, and the VIII group metal is selected from at least one of Co and Ni; wherein when the hydrogenation catalyst is analyzed by XPS spectrum, the molar ratio of the VIB group metal in the +4 valence state to the total amount of the VIB group metal is 60%~90%.

13. The method according to claim 6, characterized in that: The filling volume ratio of the silicon scavenger to the first hydrogenation catalyst in the second hydrogenation zone is 6:1-1:

6.

14. The method according to claim 6, characterized in that: The operating conditions of the hydrogenation zone II are: pressure 1.0~8.0MPa, with hydrogen partial pressure accounting for 40%~70% of the total pressure; volume space velocity 0.1~10.0h -1 The reaction temperature is 80~180℃, and the volume ratio of hydrogen to oil is 10:1~400:

1.

15. The method according to claim 14, characterized in that: The operating conditions of the hydrogenation zone II are: pressure 2.0~6.0MPa, volume space velocity 0.5~6.0h -1 , reaction temperature 100~150℃, hydrogen-oil volume ratio 100:1~200:

1.

16. The method according to claim 6, characterized in that: The third hydrogenation catalyst loaded in the hydrogenation zone 3 is a hydrodenitrogenation catalyst. The operating conditions of the hydrogenation zone 3 are: pressure 1.0~10.0MPa, volume space velocity 0.1~8.0h -1 , reaction temperature 80~220℃.

17. The method according to claim 16, characterized in that: The operating conditions of the hydrogenation zone 3 are: pressure 3.0~8.0MPa, volume space velocity 0.5~6.0h -1 , reaction temperature 120~200℃.