A double-layer electrospinning supported polymer-stabilized liquid crystal composite film
By stabilizing the liquid crystal composite film with a five-layer structure of double-layer electrospinning polymer support and optimizing the composition and structure of the liquid crystal composite layer, it solves the problems of high driving voltage, short service life and long response time in liquid crystal display devices, achieving lower driving voltage and shorter response time.
Patent Information
- Application Number
- CN202310066560.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-01-15
AI Technical Summary
The driving voltage of the liquid crystal composite film in the existing liquid crystal display device is relatively high, the service life is short, and the response time needs to be improved.
A double-layer electrospun polymer-stabilized liquid crystal composite film with a five-layer structure, including one-side loaded indium tin oxide colorless transparent polycarbonate film, nematic liquid crystal, liquid crystal anchoring network, UV absorber, and photoinitiator and nanofiber films, prepared through an electrospinning process to optimize the composition and structure of the liquid crystal composite layer.
The driving voltage of the liquid crystal composite film is reduced, the service life is extended, the response time is significantly reduced, and the gradient display performance is improved.
Smart Images

Figure CN116039210B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of liquid crystal display devices, and in particular to a double-layer electrospinning supported polymer stabilized liquid crystal composite film. Background Art
[0002] Liquid crystal (LC) has been widely used in display devices due to its electro-optical properties. Therefore, the research on LC device applications in the high-frequency range has also attracted considerable attention.
[0003] However, the driving voltage of the liquid crystal composite film in current liquid crystal display devices is usually high, the service life needs to be improved, and the response time of the display device needs to be improved.
[0004] Therefore, there is an urgent need for a liquid crystal composite film for a liquid crystal display device that can reduce the driving voltage of the liquid crystal composite film, extend the service life of the liquid crystal composite film, and reduce the response time. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a double-layer electrospinning supported polymer stabilized liquid crystal composite film which can reduce the driving voltage of the liquid crystal composite film, extend the service life of the liquid crystal composite film and reduce the response time.
[0006] In order to achieve the above object, the present invention specifically adopts the following technical solutions:
[0007] A double-layer electrospinning supported polymer stabilized liquid crystal composite film, characterized in that: it comprises five layers arranged in sequence, the first layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side;
[0008] The second layer structure is a first liquid crystal composite layer, the first liquid crystal composite layer includes nematic liquid crystal A, liquid crystal anchoring network A, ultraviolet absorber A, photoinitiator A, nanofiber film obtained by electrostatic spinning process, and spacer particles; the first liquid crystal composite layer includes the following raw materials in parts by weight: 50-80 parts of nematic liquid crystal A, 10-40 parts of liquid crystal anchoring network A, 5-10 parts of ultraviolet absorber A, 0.2-1 parts of photoinitiator A, 10-40 parts of nanofiber film, and 0.5-2 parts of spacer particles;
[0009] The nematic phase liquid crystal A comprises the following raw materials in parts by weight: 60 to 90 parts of the mother nematic phase liquid crystal A, 1 to 15 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 5 to 20 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 10 to 15 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester;
[0010] The saturation voltage of the parent nematic liquid crystal A is 25-60V, the clearing point is 60-100°C, and the viscosity is 20-80mm 2 ·s -1 , density is 5~25g / cm 3 ;
[0011] The liquid crystal anchoring network A is formed by in-situ polymerization of monomers, and the monomers are obtained from the following raw materials in parts by weight: 10 to 20 parts of 2-(trimethylsilyloxy)ethyl methacrylate, 10 to 15 parts of neopentyl glycol diacrylate, and 3 to 8 parts of 2-ethylhexyl 2-cyano-3,3-diphenyl acrylate;
[0012] The ultraviolet absorber A comprises the following raw materials in parts by weight: 0.1 to 1 part of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 0.1 to 1 part of 2-hydroxy-4-dodecyloxybenzophenone, and 0.1 to 1 part of 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazine)5-octyloxyphenol;
[0013] The photoinitiator A comprises the following raw materials in parts by weight: 0.2 to 2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.5 to 1 parts of 2-hydroxy-2-methyl-1-phenyl ketone, 0.05 to 0.5 parts of benzoin ether, and 0.1 to 1 parts of tin oxide;
[0014] The third layer structure is an ultra-thin film, the ultra-thin film has a thickness of 1 to 10 μm, a light transmittance of 90 to 99%, and a stiffness of 1 to 20 g·cm;
[0015] The fourth layer structure is a second liquid crystal composite layer, the second liquid crystal composite layer includes nematic liquid crystal B, liquid crystal anchoring network B, ultraviolet absorber B, photoinitiator B, nanofiber film obtained by electrostatic spinning process, and spacer particles; the second liquid crystal composite layer includes the following raw materials in parts by weight: 60 to 85 parts of nematic liquid crystal B, 8 to 30 parts of liquid crystal anchoring network B, 0.1 to 1 parts of ultraviolet absorber B, 0.1 to 2 parts of photoinitiator B, 10 to 40 parts of nanofiber film, and 0.5 to 5 parts of spacer particles;
[0016] The nematic liquid crystal B comprises the following raw materials in parts by weight: 50-90 parts of mother nematic liquid crystal B, 1-20 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 5-50 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 20-60 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester;
[0017] The saturation voltage of the parent nematic liquid crystal B is 5 to 15 V, the refractive index is 0.15 to 1.5, the clearing point is 60 to 150° C., and the viscosity is 10 to 35 mm 2 ·s -1 ;
[0018] The liquid crystal anchoring network B is formed by in-situ polymerization of monomers, and the monomers are obtained from the following raw materials in parts by weight: 8 to 25 parts of triethylene glycol dimethacrylate, 15 to 20 parts of trimethylolpropane trimethacrylate, and 5 to 15 parts of 3,5,5-trimethylhexyl propionate;
[0019] The ultraviolet absorber B comprises the following raw materials in parts by weight: 0.1 to 1 part of phenyl o-hydroxybenzoate, 0.1 to 1 part of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 0.1 to 1 part of 2-hydroxy-4-n-octyloxybenzophenone;
[0020] The photoinitiator B comprises the following raw materials in parts by weight: 0.2 to 2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.5 to 1 parts of 2-hydroxy-2-methyl-1-phenyl ketone, and 0.5 to 1 parts of titanium oxide;
[0021] The fifth layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side.
[0022] Furthermore, the nanofiber film has a thickness of 5 to 30 μm and a fiber diameter of 50 to 500 nm.
[0023] Furthermore, the nanofiber film comprises the following raw materials in parts by weight: 1 to 5 parts of gelatin, 1 to 10 parts of sodium alginate, 5 to 30 parts of polyvinyl alcohol, 0.1 to 2 parts of yttrium oxide and 15 to 30 parts of anhydrous ethanol.
[0024] Furthermore, the ultra-thin film comprises the following raw materials in parts by weight: 40 to 50 parts of polycarbonate, 1 to 10 parts of polypropylene, 1 to 5 parts of polyethylene, and 1 to 5 parts of polybutadiene.
[0025] Furthermore, the single-side loaded indium tin oxide colorless transparent polycarbonate film has a transmittance of 85-98%, a thickness of 50-180 μm, and a resistivity of 5-550 Ω / cm.
[0026] Furthermore, the single-sided indium tin oxide-loaded colorless transparent polycarbonate film comprises the following raw materials in parts by weight: 50 to 80 parts of polycarbonate film, 1 to 5 parts of polycaprolactone, 1 to 10 parts of polymethyl methacrylate, and 0.1 to 1 part of nano zinc oxide.
[0027] In summary, the present invention has the following beneficial effects:
[0028] The five-layer composite film of the present invention is specially designed with a first liquid crystal composite layer and a second liquid crystal composite layer of double-layer different liquid crystal structures, so that the composite film has a lower driving voltage, a shorter response time, and a better gradient display. The addition of the nanofiber film obtained by the electrostatic spinning process enhances the anchoring effect of the original liquid crystal anchoring network, making it more economical. The addition of the ultraviolet absorber A in the first liquid crystal composite layer and the ultraviolet absorber B in the second liquid crystal composite layer makes the use performance of the composite film more excellent. The addition of the ultraviolet absorber and the photoinitiator can improve the service life of the composite film.
[0029] Different compound monomers are added to the liquid crystal system of nematic phase liquid crystal A and nematic phase liquid crystal B in the raw materials. The monomers cooperate with each other to effectively reduce the saturation voltage of the liquid crystal system, reduce the viscosity of the system, and have better compatibility;
[0030] The polymerizable monomers selected for the liquid crystal anchoring network A and the liquid crystal anchoring network B in the raw materials have excellent compatibility with their respective liquid crystal systems, and under ultraviolet light polymerization, have a more uniform network texture, so that the liquid crystal droplets have a better morphology.
[0031] The polymer network formed by the multipolymer used in the nanofiber film in the raw material has a stronger anchoring effect. When combined with the ultraviolet absorbers A and B, the reaction time can be shortened. The proportion disclosed in the present invention can achieve batch matching of the refractive index of the liquid crystal and the polymer network. The response time refers to the time of light-dark change, which refers to the speed of light-dark switching. The addition of the nanofiber film effectively reduces the response time of the composite film.
[0032] The composite film of the present invention adopts an ultra-thin film as a spacer layer. The ultra-thin film of the present invention has high stiffness and is convenient for production and use.
[0033] The system selected for the single-sided indium tin oxide-loaded colorless transparent polycarbonate film of the present invention can enhance the light transmittance of the original base film and at the same time enhance the mechanical properties of the polycarbonate film, so that the polycarbonate film will not produce wrinkles during the production process, thereby producing a high-quality composite film. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic diagram of the overall structure of a double-layer electrospinning supported polymer-stabilized liquid crystal composite film of the present invention;
[0035] Figure 2 The graphs are photoelectric test curves of the liquid crystal composite films in various embodiments of the present invention and various comparative examples;
[0036] Figure 3 This is the SEM image of the nanofiber film prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0037] The specific contents of the present invention are further explained in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the conventional conditions or the conditions recommended by the manufacturer are followed. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.
[0038] The mother nematic liquid crystal A and the mother nematic liquid crystal B used in the preparation examples of the present invention are both LC-1717.
[0039] Preparation Example of the First Liquid Crystal Composite Layer
[0040] Preparation Example 1
[0041] A method for preparing a first liquid crystal composite layer comprises the following steps:
[0042] 50 parts of nematic liquid crystal A, 10 parts of liquid crystal anchoring network A, 5 parts of ultraviolet absorber A, 0.2 parts of photoinitiator A, and 0.5 parts of spacer particles were mixed, stirred for 30 minutes, and ultrasonicated for 1 hour to obtain a mixed coating, which was then coated on 10 parts of nanofiber film.
[0043] The preparation method of the nematic phase liquid crystal A comprises the following steps: mixing 60 parts of the parent nematic phase liquid crystal A, 1 part of 4-allyloxybenzoyloxybiphenyl cyanoester, 5 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 10 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester, and shaking for 20 minutes to obtain the nematic phase liquid crystal A;
[0044] The saturation voltage of the parent nematic phase liquid crystal A is 25V, the clearing point is 60℃, and the viscosity is 20mm 2 ·s -1 , density is 5g / cm 3 .
[0045] Liquid crystal anchoring network A is prepared by in-situ polymerization of monomers. 10 parts of 2-(trimethylsilyloxy)ethyl methacrylate, 10 parts of neopentyl glycol diacrylate, and 3 parts of 2-ethylhexyl 2-cyano-3,3-diphenylacrylate are taken; the raw materials are mixed and shaken for 10 minutes to obtain a monomer, which is synthesized by in-situ polymerization and cured under a UV irradiator for 10 minutes to obtain a liquid crystal anchoring network A. The curing temperature is 25°C and the curing strength is 15 mw / cm 2 .
[0046] Ultraviolet absorber A is prepared by mixing 0.1 parts of phenyl o-hydroxybenzoate, 0.1 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 0.1 parts of 2-hydroxy-4-n-octyloxybenzophenone, and 0.1 parts of 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)5-octyloxyphenol] and stirring for 10 minutes.
[0047] Photoinitiator A was prepared by mixing 0.2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.5 parts of 2-hydroxy-2-methyl-1-phenylmethanone, 0.05 parts of benzoin ether, and 0.1 parts of tin oxide and stirring for 20 minutes.
[0048] The preparation method of the nanofiber film is as follows: 1 part of gelatin, 1 part of sodium alginate, 5 parts of polyvinyl alcohol, 0.1 part of yttrium oxide and 15 parts of anhydrous ethanol are prepared into a precursor solution and then stirred at 60°C for 4 hours; the precursor solution is spun in an electrospinning machine at a spinning voltage of 20 kV and a spinning temperature of 25°C for 5 minutes to obtain a nanofiber film with a nanofiber web thickness of 5 μm and a fiber diameter of 50 nm.
[0049] Preparation Example 2
[0050] A method for preparing a first liquid crystal composite layer comprises the following steps:
[0051] 65 parts of nematic liquid crystal A, 25 parts of liquid crystal anchoring network A, 7 parts of ultraviolet absorber A, 0.5 parts of photoinitiator A, and 1 part of spacer particles were mixed, stirred for 30 minutes, and ultrasonicated for 1 hour to obtain a mixed coating, which was then applied to 20 parts of nanofiber film.
[0052] The preparation method of the nematic phase liquid crystal A comprises the following steps: mixing 75 parts of the parent nematic phase liquid crystal A, 10 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 15 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 13 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester, and shaking for 20 minutes to obtain the nematic phase liquid crystal A;
[0053] The saturation voltage of the parent nematic phase liquid crystal A is 40V, the clearing point is 80℃, and the viscosity is 60mm 2 ·s -1 , density is 15g / cm 3 .
[0054] Liquid crystal anchoring network A is prepared by in-situ polymerization of monomers. 15 parts of 2-(trimethylsilyloxy)ethyl methacrylate, 13 parts of neopentyl glycol diacrylate, and 5 parts of 2-ethylhexyl 2-cyano-3,3-diphenylacrylate are taken; the raw materials are mixed and shaken for 10 minutes to obtain a monomer, which is synthesized by in-situ polymerization and cured under a UV irradiator for 10 minutes to obtain a liquid crystal anchoring network A. The curing temperature is 25°C and the curing strength is 15 mw / cm 2 .
[0055] Ultraviolet absorber A is prepared by mixing 0.5 parts of phenyl o-hydroxybenzoate, 0.5 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 0.5 parts of 2-hydroxy-4-n-octyloxybenzophenone, and 0.5 parts of 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)5-octyloxyphenol] and stirring for 10 minutes.
[0056] Photoinitiator A was prepared by mixing 1 part of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.7 parts of 2-hydroxy-2-methyl-1-phenyl ketone, 0.3 parts of benzoin ether, and 0.5 parts of tin oxide and stirring for 20 minutes.
[0057] The preparation method of the nanofiber film is as follows: 3 parts of gelatin, 5 parts of sodium alginate, 20 parts of polyvinyl alcohol, 1 part of yttrium oxide and 20 parts of anhydrous ethanol are made into a precursor solution and then stirred at 60°C for 4 hours; the precursor solution is spun in an electrospinning machine at a spinning voltage of 20 kV and a spinning temperature of 25°C for 5 minutes to obtain a nanofiber film with a nanofiber web thickness of 20 μm and a fiber diameter of 150 nm.
[0058] Preparation Example 3
[0059] A method for preparing a first liquid crystal composite layer comprises the following steps:
[0060] 80 parts of nematic liquid crystal A, 40 parts of liquid crystal anchoring network A, 10 parts of ultraviolet absorber A, 1 part of photoinitiator A, and 2 parts of spacer particles were mixed, stirred for 30 minutes, and ultrasonicated for 1 hour to obtain a mixed coating, which was then coated on 40 parts of nanofiber film.
[0061] The preparation method of the nematic phase liquid crystal A comprises the following steps: mixing 90 parts of the parent nematic phase liquid crystal A, 15 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 20 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 15 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester, and shaking for 20 minutes to obtain the nematic phase liquid crystal A;
[0062] The saturation voltage of the parent nematic phase liquid crystal A is 60V, the clearing point is 100℃, and the viscosity is 80mm2 ·s -1 , density is 25g / cm 3 .
[0063] Liquid crystal anchoring network A is prepared by in-situ polymerization of monomers. 20 parts of 2-(trimethylsilyloxy)ethyl methacrylate, 15 parts of neopentyl glycol diacrylate, and 8 parts of 2-ethylhexyl 2-cyano-3,3-diphenylacrylate are taken; the raw materials are mixed and shaken for 10 minutes to obtain a monomer, which is synthesized by in-situ polymerization and cured under a UV irradiator for 10 minutes to obtain a liquid crystal anchoring network A. The curing temperature is 25°C and the curing strength is 15 mw / cm 2 .
[0064] Ultraviolet absorber A is prepared by mixing 1 part of phenyl o-hydroxybenzoate, 1 part of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 1 part of 2-hydroxy-4-n-octyloxybenzophenone, and 1 part of 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)5-octyloxyphenol] and stirring for 10 minutes.
[0065] Photoinitiator A was prepared by mixing 2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 1 part of 2-hydroxy-2-methyl-1-phenyl ketone, 0.5 parts of benzoin ether, and 1 part of tin oxide and stirring for 20 minutes.
[0066] The preparation method of the nanofiber film is as follows: 5 parts of gelatin, 10 parts of sodium alginate, 30 parts of polyvinyl alcohol, 2 parts of yttrium oxide and 30 parts of anhydrous ethanol are made into a precursor solution and then stirred at 60°C for 4 hours; the precursor solution is spun in an electrospinning machine at a spinning voltage of 20 kV and a spinning temperature of 25°C for 5 minutes to obtain a nanofiber film with a nanofiber web thickness of 30 μm and a fiber diameter of 500 nm.
[0067] Preparation of the second liquid crystal composite layer
[0068] Preparation Example 4
[0069] A method for preparing a second liquid crystal composite layer comprises the following steps:
[0070] 60 parts of nematic liquid crystal B, 8 parts of liquid crystal anchoring network B, 0.1 parts of ultraviolet absorber B, 0.1 parts of photoinitiator B, and 0.5 parts of spacer particles were mixed, stirred for 30 minutes, and ultrasonicated for 1 hour to obtain a mixed coating, which was then applied on 10 parts of nanofiber film.
[0071] The preparation method of the nematic phase liquid crystal B comprises the following steps: 50 parts of the parent nematic phase liquid crystal B, 1 part of 4-allyloxybenzoyloxybiphenyl cyanoester, 5 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 20 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester are mixed, and the mixture is shaken for 20 minutes to obtain the nematic phase liquid crystal B;
[0072] The saturation voltage of the parent nematic liquid crystal B is 5V, the refractive index is 0.15, the clearing point is 60℃, and the viscosity is 10mm 2 ·s -1 .
[0073] Liquid crystal anchoring network B is prepared by in-situ polymerization of monomers. 8 parts of triethylene glycol dimethacrylate, 15 parts of trimethylolpropane trimethacrylate, and 5 parts of 3,5,5-trimethylhexyl propionate are taken; the raw materials are mixed and shaken for 10 minutes to obtain monomers. After in-situ polymerization synthesis, the liquid crystal anchoring network A is obtained by curing under a UV irradiator for 10 minutes. The curing temperature is 25°C and the curing strength is 15mw / cm 2 .
[0074] Ultraviolet absorber B is prepared by mixing 0.1 parts of phenyl o-hydroxybenzoate, 0.1 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 0.1 parts of 2-hydroxy-4-n-octyloxybenzophenone and stirring for 10 minutes.
[0075] Photoinitiator B was prepared by mixing 0.2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.5 parts of 2-hydroxy-2-methyl-1-phenylmethanone, and 0.5 parts of titanium oxide and stirring for 20 minutes.
[0076] The preparation method of the nanofiber film is as follows: 1 part of gelatin, 1 part of sodium alginate, 5 parts of polyvinyl alcohol, 0.1 part of yttrium oxide and 15 parts of anhydrous ethanol are prepared into a precursor solution and then stirred at 60°C for 4 hours; the precursor solution is spun in an electrospinning machine at a spinning voltage of 20 kV and a spinning temperature of 25°C for 5 minutes to obtain a nanofiber film with a nanofiber web thickness of 5 μm and a fiber diameter of 50 nm.
[0077] Preparation Example 5
[0078] A method for preparing a second liquid crystal composite layer comprises the following steps:
[0079] 75 parts of nematic liquid crystal B, 15 parts of liquid crystal anchoring network B, 0.5 parts of ultraviolet absorber B, 1 part of photoinitiator B, and 3 parts of spacer particles were mixed, stirred for 30 minutes, and ultrasonicated for 1 hour to obtain a mixed coating, which was then applied to 25 parts of nanofiber film.
[0080] The preparation method of the nematic phase liquid crystal B comprises the following steps: 80 parts of the parent nematic phase liquid crystal B, 10 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 25 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 40 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester are mixed, and the mixture is shaken for 20 minutes to obtain the nematic phase liquid crystal B;
[0081] The saturation voltage of the parent nematic liquid crystal B is 10V, the refractive index is 0.8, the clearing point is 100℃, and the viscosity is 25mm 2 ·s -1 .
[0082] Liquid crystal anchoring network B is prepared by in-situ polymerization of monomers. 15 parts of triethylene glycol dimethacrylate, 17 parts of trimethylolpropane trimethacrylate, and 10 parts of 3,5,5-trimethylhexyl propionate are taken; the raw materials are mixed and shaken for 10 minutes to obtain monomers. After in-situ polymerization synthesis, the liquid crystal anchoring network A is obtained by curing under a UV irradiator for 10 minutes. The curing temperature is 25°C and the curing strength is 15mw / cm 2 .
[0083] Ultraviolet absorber B is prepared by mixing 0.5 parts of phenyl o-hydroxybenzoate, 0.5 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 0.5 parts of 2-hydroxy-4-n-octyloxybenzophenone and stirring for 10 minutes.
[0084] Photoinitiator B was prepared by mixing 1 part of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.7 parts of 2-hydroxy-2-methyl-1-phenylmethanone, and 0.7 parts of titanium oxide and stirring for 20 minutes.
[0085] The preparation method of the nanofiber film is as follows: 3 parts of gelatin, 5 parts of sodium alginate, 20 parts of polyvinyl alcohol, 1 part of yttrium oxide and 20 parts of anhydrous ethanol are made into a precursor solution and then stirred at 60°C for 4 hours; the precursor solution is spun in an electrospinning machine at a spinning voltage of 20 kV and a spinning temperature of 25°C for 5 minutes to obtain a nanofiber film with a nanofiber web thickness of 20 μm and a fiber diameter of 150 nm.
[0086] Preparation Example 6
[0087] A method for preparing a second liquid crystal composite layer comprises the following steps:
[0088] 85 parts of nematic liquid crystal B, 30 parts of liquid crystal anchoring network B, 1 part of ultraviolet absorber B, 2 parts of photoinitiator B, and 5 parts of spacer particles were mixed, stirred for 30 minutes, and ultrasonicated for 1 hour to obtain a mixed coating, which was then applied on 40 parts of nanofiber film.
[0089] The preparation method of the nematic phase liquid crystal B comprises the following steps: 90 parts of the parent nematic phase liquid crystal B, 20 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 50 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 60 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester are mixed, and the mixture is shaken for 20 minutes to obtain the nematic phase liquid crystal B;
[0090] The saturation voltage of the parent nematic liquid crystal B is 15V, the refractive index is 1.5, the clearing point is 150℃, and the viscosity is 35mm 2 ·s -1 .
[0091] Liquid crystal anchoring network B is prepared by in-situ polymerization of monomers. 25 parts of triethylene glycol dimethacrylate, 20 parts of trimethylolpropane trimethacrylate, and 15 parts of 3,5,5-trimethylhexyl propionate are taken; the raw materials are mixed and shaken for 10 minutes to obtain monomers. After in-situ polymerization synthesis, the liquid crystal anchoring network A is obtained by curing under a UV irradiator for 10 minutes. The curing temperature is 25°C and the curing strength is 15mw / cm 2 .
[0092] Ultraviolet absorber B is prepared by mixing 1 part of phenyl o-hydroxybenzoate, 1 part of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 1 part of 2-hydroxy-4-n-octyloxybenzophenone and stirring for 10 minutes.
[0093] Photoinitiator B was prepared by mixing 2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 1 part of 2-hydroxy-2-methyl-1-phenyl ketone, and 1 part of titanium oxide and stirring for 20 minutes.
[0094] The preparation method of the nanofiber film is as follows: 5 parts of gelatin, 10 parts of sodium alginate, 30 parts of polyvinyl alcohol, 2 parts of yttrium oxide and 30 parts of anhydrous ethanol are made into a precursor solution and then stirred at 60°C for 4 hours; the precursor solution is spun in an electrospinning machine at a spinning voltage of 20 kV and a spinning temperature of 25°C for 5 minutes to obtain a nanofiber film with a nanofiber web thickness of 30 μm and a fiber diameter of 500 nm.
[0095] Example
[0096] Example 1
[0097] A double-layer electrospinning supported polymer stabilized liquid crystal composite film, referring to Figure 1 , including five layers arranged in sequence:
[0098] The first layer structure is a colorless transparent polycarbonate film loaded with indium tin oxide on one side, and the film thickness is 50μm, the light transmittance is 85%, and the resistivity is 5Ω / cm;
[0099] The second layer structure is a first color liquid crystal composite layer prepared by the method in Preparation Example 1,
[0100] The third layer is a light-transmitting film with a thickness of 1 μm, a light transmittance of 90%, and a stiffness of 1 g·cm.
[0101] The fourth layer structure is a second color liquid crystal composite layer prepared by the method in Preparation Example 4.
[0102] The fifth layer structure is a colorless transparent polycarbonate film loaded with indium tin oxide on one side, and the film thickness is 50 μm, the light transmittance is 85%, and the resistivity is 5Ω / cm;
[0103] The first layer structure, the second layer structure, the third layer structure and the fourth layer structure are pressed into one body and then bonded to the fifth layer structure by glue.
[0104] The preparation method of the colorless transparent polycarbonate film comprises the following steps: heating 40 parts of polycarbonate film to 200°C, then adding 1 part of polycaprolactone, 1 part of polymethyl methacrylate, and 0.1 part of nano zinc oxide while stirring, continuing stirring for 2 hours, cooling to 250°C to obtain a mixture A, and blow molding the mixture A to form a colorless transparent polycarbonate film.
[0105] The preparation method of the ultra-thin film includes the following steps: heating 50 parts of polycarbonate to 250°C, then adding 1 part of polypropylene, 1 part of polyethylene, and 1 part of polybutadiene, stirring continuously for 1.5 hours, cooling to 225°C to obtain a mixture B, and blow molding the mixture B to form an ultra-thin film.
[0106] Example 2
[0107] A double-layer electrospinning supported polymer-stabilized liquid crystal composite film comprises five layers arranged in sequence:
[0108] The first layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side, and the film thickness is 100μm, the light transmittance is 93%, and the resistivity is 300Ω / cm;
[0109] The second layer structure is a first color liquid crystal composite layer prepared by the method in Preparation Example 1,
[0110] The third layer is a light-transmitting film with a thickness of 5 μm, a light transmittance of 95%, and a stiffness of 5 g·cm.
[0111] The fourth layer structure is a second color liquid crystal composite layer prepared by the method in Preparation Example 4.
[0112] The fifth layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side, and the film thickness is 100 μm, the light transmittance is 93%, and the resistivity is 300 Ω / cm.
[0113] The first layer structure, the second layer structure, the third layer structure and the fourth layer structure are pressed into one body and then bonded to the fifth layer structure by glue.
[0114] The preparation method of the colorless transparent polycarbonate film comprises the following steps: heating 50 parts of polycarbonate film to 200°C, then adding 1 part of polycaprolactone, 1 part of polymethyl methacrylate, and 0.1 part of nano zinc oxide while stirring, continuing stirring for 2 hours, cooling to 250°C to obtain a mixture A, and blow molding the mixture A to form a colorless transparent polycarbonate film.
[0115] The preparation method of the ultra-thin film includes the following steps: heating 50 parts of polycarbonate to 250°C, then adding 5 parts of polypropylene, 3 parts of polyethylene, and 3 parts of polybutadiene, continuously stirring for 1.5 hours, cooling to 225°C to obtain a mixture B, and blow molding the mixture B to form an ultra-thin film.
[0116] Example 3
[0117] A double-layer electrospinning supported polymer-stabilized liquid crystal composite film comprises five layers arranged in sequence:
[0118] The first layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side, and the film thickness is 150μm, the light transmittance is 98%, and the resistivity is 550Ω / cm;
[0119] The second layer structure is a first color liquid crystal composite layer prepared by the method in Preparation Example 1,
[0120] The third layer is a light-transmitting film with a thickness of 10 μm, a light transmittance of 99%, and a stiffness of 20 g·cm.
[0121] The fourth layer structure is a second color liquid crystal composite layer prepared by the method in Preparation Example 4.
[0122] The fifth layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side, and the film thickness is 150 μm, the light transmittance is 98%, and the resistivity is 550 Ω / cm.
[0123] The first layer structure, the second layer structure, the third layer structure and the fourth layer structure are pressed into one body and then bonded to the fifth layer structure by glue.
[0124] The preparation method of the colorless transparent polycarbonate film comprises the following steps: 80 parts of polycarbonate film, 5 parts of polycaprolactone, 10 parts of polymethyl methacrylate, and 1 part of nano zinc oxide are continuously stirred for 2 hours, cooled to 250°C to obtain a mixture A, and the mixture A is blow-molded to form a colorless transparent polycarbonate film.
[0125] The preparation method of the ultra-thin film includes the following steps: heating 45 parts of polycarbonate to 250°C, then adding 10 parts of polypropylene, 5 parts of polyethylene, and 5 parts of polybutadiene, continuously stirring for 1.5 hours, cooling to 225°C to obtain a mixture B, and blow molding the mixture B to form an ultra-thin film.
[0126] Comparative Example
[0127] Comparative Example 1
[0128] A double-layer electrospinning supported polymer stabilized liquid crystal composite film is produced according to the method in Example 1, except that no nanofiber film is added to the first liquid crystal composite layer.
[0129] Comparative Example 2
[0130] A double-layer electrospinning supported polymer stabilized liquid crystal composite film is produced according to the method in Example 1, except that there is no second liquid crystal composite layer.
[0131] Comparative Example 3
[0132] A double-layer electrospinning supported polymer stabilized liquid crystal composite film is prepared according to the method in Example 1, except that no nanofiber film is added to the second liquid crystal composite layer.
[0133] Performance Testing
[0134] The contrast, response time, driving voltage (V10), saturation voltage (V90) and UV shielding performance of the composite films in the above-mentioned embodiments and comparative examples were tested. The test results are shown in Table 1.
[0135] Table 1:
[0136]
[0137] Figure 2 The photoelectric test curve diagram of the electrospinning supported polymer stabilized liquid crystal composite film prepared in Examples 1-3 of the present invention and Comparative Examples 1-3 shows that compared with Comparative Examples 1-3, the driving voltages of Examples 1-3 of the present invention are 30.4V, 30.9V and 32.4V, respectively, which are significantly lower than Comparative Examples 1-3, indicating that the liquid crystal composite film in the present invention can effectively reduce the driving voltage.
[0138] Figure 3This is a SEM image of the nanofiber film in Preparation Example 1 of the present invention. It can be seen that the nanofiber film forms a stable network structure with multiple polymers.
Claims
1. A double-layer electrospinning supported polymer-stabilized liquid crystal composite film, characterized in that: It includes five layers of structures arranged in sequence, the first layer of which is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side; The second layer structure is a first liquid crystal composite layer, the first liquid crystal composite layer includes nematic liquid crystal A, liquid crystal anchoring network A, ultraviolet absorber A, photoinitiator A, nanofiber film obtained by electrostatic spinning process, and spacer particles; the first liquid crystal composite layer includes the following raw materials in parts by weight: 50-80 parts of nematic liquid crystal A, 10-40 parts of liquid crystal anchoring network A, 5-10 parts of ultraviolet absorber A, 0.2-1 parts of photoinitiator A, 10-40 parts of nanofiber film, and 0.5-2 parts of spacer particles; The nematic phase liquid crystal A comprises the following raw materials in parts by weight: 60 to 90 parts of the mother nematic phase liquid crystal A, 1 to 15 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 5 to 20 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 10 to 15 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester; The saturation voltage of the parent nematic liquid crystal A is 25-60V, the clearing point is 60-100°C, and the viscosity is 20-80mm 2 ·s -1 , density is 5~25g / cm 3 ; The liquid crystal anchoring network A is formed by in-situ polymerization of monomers, and the monomers are obtained from the following raw materials in parts by weight: 10 to 20 parts of 2-(trimethylsilyloxy)ethyl methacrylate, 10 to 15 parts of neopentyl glycol diacrylate, and 3 to 8 parts of 2-ethylhexyl 2-cyano-3,3-diphenyl acrylate; The ultraviolet absorber A comprises the following raw materials in parts by weight: 0.1 to 1 part of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 0.1 to 1 part of 2-hydroxy-4-dodecyloxybenzophenone, 0.1 to 1 part of 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)5-octyloxyphenol; The photoinitiator A comprises the following raw materials in parts by weight: 0.2 to 2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.5 to 1 parts of 2-hydroxy-2-methyl-1-phenyl ketone, 0.05 to 0.5 parts of benzoin ether, and 0.1 to 1 parts of tin oxide; The third layer structure is an ultra-thin film, the ultra-thin film has a thickness of 1 to 10 μm, a light transmittance of 90 to 99%, and a stiffness of 1 to 20 g·cm; The fourth layer structure is a second liquid crystal composite layer, wherein the second liquid crystal composite layer includes nematic liquid crystal B, liquid crystal anchoring network B, ultraviolet absorber B, photoinitiator B, nanofiber film obtained by electrospinning process, and spacer particles; The second liquid crystal composite layer comprises the following raw materials in parts by weight: 60 to 85 parts of nematic liquid crystal B, 8 to 30 parts of liquid crystal anchoring network B, 0.1 to 1 parts of ultraviolet absorber B, 0.1 to 2 parts of photoinitiator B, 10 to 40 parts of nanofiber film, and 0.5 to 5 parts of spacer particles; The nematic liquid crystal B comprises the following raw materials in parts by weight: 50-90 parts of mother nematic liquid crystal B, 1-20 parts of 4-allyloxybenzoyloxybiphenyl cyanoester, 5-50 parts of 4-allyloxyphenylpropionyloxybiphenyl cyanoester, and 20-60 parts of 9-(4-(4-allyloxy)benzoyloxyphenyl)oxycarbonylnonanoyloxybiphenyl cyanoester; The saturation voltage of the parent nematic liquid crystal B is 5 to 15 V, the refractive index is 0.15 to 1.5, the clearing point is 60 to 150° C., and the viscosity is 10 to 35 mm 2 ·s -1 ; The liquid crystal anchoring network B is formed by in-situ polymerization of monomers, and the monomers are obtained from the following raw materials in parts by weight: 8 to 25 parts of triethylene glycol dimethacrylate, 15 to 20 parts of trimethylolpropane trimethacrylate, and 5 to 15 parts of 3,5,5-trimethylhexyl propionate; The ultraviolet absorber B comprises the following raw materials in parts by weight: 0.1 to 1 part of phenyl o-hydroxybenzoate, 0.1 to 1 part of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 0.1 to 1 part of 2-hydroxy-4-n-octyloxybenzophenone; The photoinitiator B comprises the following raw materials in parts by weight: 0.2 to 2 parts of 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 0.5 to 1 parts of 2-hydroxy-2-methyl-1-phenyl ketone, and 0.5 to 1 parts of titanium oxide; The fifth layer structure is a colorless and transparent polycarbonate film loaded with indium tin oxide on one side.
2. A double-layer electrospun supported polymer-stabilized liquid crystal composite film according to claim 1, characterized in that: The thickness of the nanofiber film is 5-30 μm, and the fiber diameter is 50-500 nm.
3. A double-layer electrospun supported polymer-stabilized liquid crystal composite film according to claim 1 or 2, characterized in that: The nanofiber film comprises the following raw materials in parts by weight: 1 to 5 parts of gelatin, 1 to 10 parts of sodium alginate, 5 to 30 parts of polyvinyl alcohol, 0.1 to 2 parts of yttrium oxide and 15 to 30 parts of anhydrous ethanol.
4. The double-layer electrospun supported polymer-stabilized liquid crystal composite film according to claim 1, characterized in that: The ultra-thin film comprises the following raw materials in parts by weight: 40 to 50 parts of polycarbonate, 1 to 10 parts of polypropylene, 1 to 5 parts of polyethylene, and 1 to 5 parts of polybutadiene.
5. The double-layer electrospun supported polymer-stabilized liquid crystal composite film according to claim 1, characterized in that: The single-side loaded indium tin oxide colorless transparent polycarbonate film has a transmittance of 85-98%, a thickness of 50-180 μm, and a resistivity of 5-550 Ω / cm.
6. A double-layer electrospun supported polymer-stabilized liquid crystal composite film according to claim 1 or 5, characterized in that: The single-side indium tin oxide-loaded colorless transparent polycarbonate film comprises the following raw materials in parts by weight: 50 to 80 parts of polycarbonate film, 1 to 5 parts of polycaprolactone, 1 to 10 parts of polymethyl methacrylate, and 0.1 to 1 part of nano zinc oxide.