A high-adhesion and high-temperature resistant PE release film for building waterproofing membrane and a manufacturing method thereof

By modifying the granulation and applying the oil-resistant coating, the temperature resistance and oil resistance of the PE release film for building waterproofing membranes are improved, the problems of poor temperature resistance and oil resistance of the existing membrane materials are solved, and the service life is extended. service life and reduced production costs.

CN116042130BActive Publication Date: 2024-10-18HUNAN YOUPERTH NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310149078.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-10-18
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

The existing PE release films used for building waterproofing have poor temperature resistance and oil resistance, which causes the film to be easily scalded during use, turn yellow during storage, and have reduced viscosity. It cannot fully exert the function of the waterproof membrane, and the PET release film has poor performance. Inconsistency in rigidity and asphalt shrinkage leads to bulging of the membrane and water leakage problems.

Method used

The masterbatch dilution method + multi-layer blown film process is used to create high temperature-resistant masterbatch through parallel twin-screw modification, and a resistive oily coating PVDC or PVA is coated on the PE release film to improve the high temperature resistance and resistance of the film. Oil performance.

Benefits of technology

Significantly improves the temperature resistance and oil resistance of the PE release film, extends the service life of the membrane, maintains the viscosity of the asphalt membrane, reduces production costs, avoids yellowing of the membrane surface, and improves the product's durability Value for money.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116042130B_ABST
    Figure CN116042130B_ABST
Patent Text Reader

Abstract

This invention belongs to the fields of building waterproofing, plastics, and adhesives, and discloses a high-adhesion, high-temperature resistant PE release film for building waterproofing membranes and its manufacturing method. The manufacturing method includes the following steps: (1) Preparation of a high-temperature resistant substrate layer: PE / PP is blended and modified with PET or PA6 and granulated to obtain a high-temperature resistant masterbatch; the high-temperature resistant masterbatch is then blended with PE raw materials in a certain proportion and blown into a multilayer film to obtain a high-temperature resistant substrate layer; (2) Preparation of an oil-resistant coating: a PVDC or PVA coating is applied to the surface of the high-temperature resistant substrate layer to obtain an oil-resistant coating; (3) Preparation of a silicone oil release layer: silicone oil is applied to the surface of the oil-resistant coating, cured and cooled to obtain the final product. This invention uses PET or PA6 blended and modified PE / PP materials to make a high-temperature resistant masterbatch, and the multilayer blown film method can significantly improve the temperature resistance of the film; at the same time, the method of applying an oil-resistant coating PVDC or PVA to the film surface improves the oil resistance of the film; and its manufacturing method is safe and environmentally friendly, with low production cost and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building waterproofing, plastics and adhesives, and relates to a PE release film, in particular to a high-adhesion and high-temperature resistant PE release film for building waterproofing coiled materials and a manufacturing method thereof. Background Art

[0002] The existing PE release film for building waterproofing has low temperature resistance and poor oil resistance, which leads to the PE release film being easily burned during the production of waterproof rolls due to temperature resistance, yellowing of the film surface due to oil resistance during storage, and decreased viscosity during use, which cannot fully play the role of waterproof rolls. When using PET release film, due to the large rigidity and bending modulus of PET release film, the roll produced is inconsistent with the shrinkage of asphalt and PET, causing the roll to bulge, and water leakage is easy to occur during construction. Therefore, how to improve the function of the existing PE release film to improve the temperature resistance and oil resistance has become a technical problem that technicians in this field need to solve urgently. Summary of the invention

[0003] Aiming at the poor temperature resistance of the existing PE film, the present invention provides a high-adhesion and high-temperature resistant PE release film for building waterproofing coiled materials and a manufacturing method thereof.

[0004] The high-adhesion and high-temperature resistant PE release film for building waterproof membrane provided by the present invention has a main solution of adopting the "masterbatch dilution method + multi-layer film blowing" process, and manufacturing the high-temperature resistant masterbatch through parallel twin-screw modified granulation; mixing the prepared masterbatch with PE raw material according to proportion, and blowing in a three-layer or more film blowing machine.

[0005] In order to significantly improve the temperature resistance of the PE release film, the coating temperature is increased from 120°C to 145°C when the silicone oil is applied, and the film is not burned at 170°C during the production of the asphalt coil. In view of the poor oil resistance of the PE film, a method of coating the film surface with an oil-resistant coating PVDC or PVA is adopted to improve the oil resistance of the film, thereby improving the yellowing resistance of the film and maintaining the viscosity of the asphalt coil.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] The first aspect of the present invention is to provide a method for manufacturing a high-adhesion and high-temperature resistant PE release film for building waterproofing membrane, comprising the following steps:

[0008] (1) Preparation of high temperature resistant substrate layer

[0009] Weigh the raw material components of high-temperature-resistant masterbatch, use PET or PA6 to blend and modify PE / PP through a parallel twin-screw extruder to obtain high-temperature-resistant masterbatch; use a three-layer or more film blowing machine to blend the high-temperature-resistant masterbatch with the PE raw material in proportion and place it in the middle layer of the film blowing, and perform multi-layer film blowing to obtain a high-temperature-resistant substrate layer;

[0010] (2) Preparation of oil-resistant coating

[0011] A coating machine is used to coat a PVDC or PVA coating on the surface of the high temperature resistant substrate layer, and the water is dried at 100-150° C. to obtain an oil-resistant coating on the surface of the high temperature resistant substrate layer;

[0012] (3) Preparation of silicone oil release layer

[0013] Continue to use the coating machine to apply silicone oil on the surface of the oil-resistant coating, solidify it at 140-150°C, and cool it to obtain a high-adhesion and high-temperature resistant PE release film with a surface layer of silicone oil release layer, a middle layer of oil-resistant coating, and a bottom layer of high-temperature substrate layer.

[0014] Preferably, in step (1), the high temperature resistant masterbatch comprises the following components in parts by weight:

[0015]

[0016] Preferably, in step (1), the high temperature resistant masterbatch comprises the following components in parts by weight:

[0017]

[0018] Preferably, the PET and / or PA6 is preferably PET; and the PP and / or HDPE is preferably PP.

[0019] Preferably, the LLDPE and / or M-LLDPE is LLDPE, and the LLDPE melt index is 1 to 4 / 10min.

[0020] Preferably, the compatibilizer is at least one of MAH-g-PE (maleic acid liver grafted PE) or GMA-g-PE (glycidyl methacrylate grafted PE).

[0021] More preferably, the compatibilizer is MAH-g-PE (maleic acid liver grafted PE).

[0022] Preferably, the high temperature resistant masterbatch comprises the following components in parts by weight:

[0023]

[0024]

[0025] Further preferably, the high temperature resistant masterbatch comprises the following components in parts by weight:

[0026]

[0027] More preferably, the high temperature resistant masterbatch further comprises an antioxidant masterbatch, and the high temperature resistant masterbatch is formed by mixing and granulating an antioxidant and a LLDPE resin;

[0028] Wherein, the weight of the antioxidant in the high temperature resistant masterbatch accounts for 25-35% of the total weight;

[0029] The antioxidant is composed of a primary antioxidant 1010 and an auxiliary antioxidant 168 in a weight ratio of 1:2.

[0030] Further preferably, the mass of the antioxidant in the high temperature resistant masterbatch accounts for 30% of the total, that is, the mass ratio of the antioxidant to the LLDPE resin is 3:7.

[0031] Preferably, in step (1), the preparation process of the high temperature resistant masterbatch is:

[0032] Raw materials of high temperature resistant masterbatch - weight loss metering, mixing and stirring - parallel twin screw granulator - granulation - drying - inspection - packaging;

[0033] Among them, granulation temperature (℃): 160, 200, 250, 260, 270, 270, 270, 260, 250; melt temperature (℃): 250; melt pressure: 4-6Mpa; rotation speed: 300-400r / min.

[0034] Preferably, in step (1), the multi-layer blown film is produced using a three-layer, five-layer or seven-layer blown film machine.

[0035] Film structure: three-layer film blowing machine

[0036]

[0037] Film structure: five-layer film blowing machine

[0038]

[0039]

[0040] Film structure: Seven-layer film blowing machine

[0041]

[0042] The film blowing process is: each layer metering - extrusion by extruder - blowing by die head - traction stretching - corona - edge cutting - film winding - rewinding and slitting according to customer requirements;

[0043] Process: Film blowing temperature

[0044]

[0045] Among them, screw speed: 60 ~ 100r / min; melt pressure: 35 ~ 50mpa; line speed: 20 ~ 40m / min.

[0046] The present invention adopts a multi-layer blown film method to complete the preparation of the high temperature resistant substrate. The blown film can be three layers or more, wherein the high temperature masterbatch + HDPE are placed in a middle layer in a certain proportion, and the proportion of the middle layer can be adjusted according to the temperature resistance requirements, such as adjusting the proportion to 50-80%; further optimization, the proportion of the high temperature resistant masterbatch is more suitable at 70%.

[0047] And because the middle layer adopts high temperature resistant masterbatch, the selection range of HDPE materials is wider. The melt flow rate of HDPE can be selected in the range of 0.05-1g / 10min, 2.16kg, 195℃. It is necessary not only to select HDPE resin with high melting point, high crystallinity and melt flow rate ≤0.1g / (10min, 2.16kg, 195℃) which is difficult to process, but also to make the processing performance of blown film better.

[0048] Preferably, in the step (2), the oil-resistant coating is coated with a PVDC emulsion prepared from the following components, in parts by weight: 40-50 parts of vinylidene chloride, 9-11 parts of sodium methacrylate sulfonate, 3-5 parts of butyl acrylate, 3-5 parts of acrylic acid, 1-2 parts of methyl methacrylate, 0.8-1.4 parts of azobisisobutyronitrile, 1-1.5 parts of polyoxyethylene ether, 0.6-0.8 parts of dimethyl silicone oil, and 23.3-32.5 parts of water.

[0049] Preferably, the oil-resistant coating is coated with a PVDC emulsion prepared from the following components, by weight: 42-48 parts of vinylidene chloride, 9.5-10.5 parts of sodium methacrylate sulfonate, 4-5 parts of butyl acrylate, 4-5 parts of acrylic acid, 1.5-2 parts of methyl methacrylate, 0.9-1.2 parts of azobisisobutyronitrile, 1.2-1.5 parts of polyoxyethylene ether, 0.7-0.8 parts of dimethyl silicone oil, and 25-30 parts of water.

[0050] More preferably, the oil-resistant coating is coated with a PVDC emulsion prepared from the following components, by weight: 45 parts of vinylidene chloride, 10 parts of sodium methacrylate, 5 parts of butyl acrylate, 5 parts of acrylic acid, 2 parts of methyl methacrylate, 1 part of azobisisobutyronitrile, 1.5 parts of polyoxyethylene ether, 0.6 parts of dimethyl silicone oil, and 29.9 parts of water.

[0051] Further preferably, the preparation method of the PVDC emulsion comprises the following steps:

[0052] (1) Weigh vinylidene chloride, sodium methacrylate, butyl acrylate, acrylic acid, methyl methacrylate, azobisisobutyronitrile, polyoxyethylene ether, dimethyl silicone oil, and water according to the formula;

[0053] (2) Add all the vinylidene chloride, sodium methacrylate sulfonate, 1 / 3 of azobisisobutyronitrile, 1 / 3 of polyoxyethylene ether and 3 / 4 of water into a reaction kettle, heat the reaction kettle to 60-65° C., and stir at 300-500 r / min for 10-15 min to obtain a mixed solution A;

[0054] (3) Then, all the butyl acrylate, acrylic acid, methyl methacrylate and the remaining water are slowly and evenly added to the reaction kettle continuously within one hour, and stirring is continued for 1 to 2 hours to obtain a mixed solution B;

[0055] (4) Add the remaining polyoxyethylene ether of azobisisobutyronitrile and all the polyoxyethylene ether and dimethyl silicone oil to the reactor in sequence, raise the temperature to 73-78° C., and stir at 200-300 r / min for 15-20 min to obtain a PVDC emulsion.

[0056] The second aspect of the present invention is to provide a high-adhesion and high-temperature resistant PE release film for building waterproofing coiled materials, comprising: a silicone oil release layer located on the surface, an oil-resistant coating located in the middle, and a high-temperature substrate layer located at the bottom;

[0057] Wherein, the oil-resistant coating is a PVDC or PVA coating; the high-temperature substrate layer is a high-temperature resistant multi-layer co-extruded film.

[0058] Preferably, the thickness of the oil-resistant coating is 0.0003-0.001 mm; the thickness of the high-temperature substrate layer is 0.025-0.04 mm.

[0059] More preferably, the oil-resistant coating is a PVDC coating, and the high-temperature substrate layer is a high-temperature resistant multi-layer co-extruded film.

[0060] Preferably, the thickness of the oil-resistant coating is 0.0005-0.0008 mm; the thickness of the high-temperature substrate layer is 0.030-0.035 mm.

[0061] Preferably, the high temperature resistant multi-layer co-extruded film comprises: a silicon coating layer located on the surface layer, at least one high temperature resistant layer located in the middle layer, and a color layer located in the bottom layer;

[0062] Wherein, the high temperature resistant layer of the middle layer is composed of a high temperature resistant masterbatch and a PE raw material, the mass fraction of the high temperature resistant masterbatch is 50-80%, and the mass fraction of the PE raw material is 20-50%.

[0063] More preferably, in the high temperature resistant layer of the middle layer, the mass fraction of the high temperature resistant masterbatch is 70%, and the mass fraction of the PE raw material is 30%.

[0064] Preferably, the silicon-coated layer of the surface layer is composed of HDPE and LLDPE, the mass fraction of the HDPE is 70-85%, and the mass fraction of the LLDPE is 15-30%.

[0065] More preferably, in the silicon-coated layer on the surface, the mass fraction of the HDPE is 75-80%, and the mass fraction of the LLDPE is 20-25%.

[0066] Preferably, the color layer of the bottom layer is composed of HDPE, LLDPE and masterbatch, the mass fraction of HDPE is 70-80%, the mass fraction of LLDPE is 15-30%, and the mass fraction of masterbatch is 5-10%.

[0067] More preferably, in the color layer of the bottom layer, the mass fraction of the HDPE is 74-76%, the mass fraction of the LLDPE is 20-25%, and the mass fraction of the masterbatch is 6-8%.

[0068] Preferably, the silicone oil material used in the silicone oil release layer is heat-curable vinyl addition reaction silicone oil, and its thickness is 0.0003-0.0006 mm.

[0069] Preferably, the thickness of the silicone oil release layer is 0.0004-0.0005 mm.

[0070] The above scheme is aimed at the defect that the existing PE film material has poor resistance to mineral oil in asphalt, so that the solvent oil in the produced coil can easily penetrate through the PE release film, thereby causing the surface of the coil to turn yellow and the adhesion performance to deteriorate. The present invention adopts a specific oil-resistant coating to greatly improve the barrier performance of the film. Its oil resistance is characterized by an oxygen permeability from the original 3000cm 3 / m 3 , 24h, 1atm, down to ≤30cm 3 / m 3 , 24h, 1at. And after 6 months of outdoor use, the surface of the coil does not turn yellow, and the adhesion retention is increased from ≤50% in the past to >80%, which greatly increases the service life of the coil.

[0071] The present invention adopts the above technical solution, which has the following technical effects compared with the prior art:

[0072] (1) The material improvement method of PET blending modified PE / PP and PA6 blending modified PE / PP is adopted to make high temperature resistant masterbatch, which significantly improves the temperature resistance of the film and overcomes the defect of poor temperature resistance of PE film; because the middle layer adopts high temperature resistant masterbatch, the selection range of HDPE material is wider, so that the processing performance of blown film is better;

[0073] (2) The coating + material improvement technology is used to improve the existing technology and equipment, overcoming the environmentally unfriendly and high cost defects of the existing multi-layer co-extrusion of more than five layers of PE / TIE / PA6 / TIE / PE (TIE represents adhesive resin); the production cost is reduced by >20%, and the product has a high cost performance ratio; and because the PE modification method is adopted, the content of PET or PA6+PVDC does not exceed 10%, according to international general practice, it is a single material and an environmentally friendly material;

[0074] (3) The oil resistance of the membrane is improved by coating the membrane surface with an oil-resistant coating of PVDC or PVA, thereby improving the yellowing resistance of the membrane and maintaining the viscosity of the asphalt coil. This overcomes the defect of the existing PE membrane's poor oil resistance and greatly improves the barrier performance of the PE membrane. Moreover, after six months of outdoor use, the surface of the coil does not turn yellow, and the adhesion retention is increased from ≤50% in the past to >80%;

[0075] (4) PE release film for building waterproofing has an annual domestic consumption of 500 million square meters. If the coating + material modification manufacturing method of the present invention is adopted, for example, the production cost of producing a 0.03 mm thick release film will drop from 0.8 yuan / square meter to 0.76 yuan, directly creating a profit of 70 million yuan, which has good social and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Figure 1 It is a schematic structural diagram of a high-adhesion and high-temperature-resistant PE release film for building waterproofing coiled materials of the present invention, in which the high-temperature-resistant substrate layer is a three-layer film layer;

[0077] Figure 2 It is a schematic structural diagram of a high-adhesion and high-temperature resistant PE release film for building waterproofing membrane of the present invention, in which the high-temperature resistant substrate layer is composed of five film layers;

[0078] Figure 3 This is a schematic structural diagram of a high-adhesion and high-temperature resistant PE release film for building waterproofing membranes of the present invention;

[0079] Figure 4 The present invention is a schematic diagram of the preparation process of a high-adhesion and high-temperature-resistant PE release film for building waterproof membrane. DETAILED DESCRIPTION

[0080] The present invention is described in detail and specifically by specific examples below to provide a better understanding of the present invention, but the following examples do not limit the scope of the present invention.

[0081] Example 1 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0082] (I) Preparation of high temperature resistant substrate layer

[0083] (1) Weigh the raw material components of high temperature resistant masterbatch respectively by weight: 30 parts of PET, 35 parts of PP or HDPE, 20 parts of LLDPE, 6 parts of GMA-g-PE, and 1.5 parts of antioxidant masterbatch;

[0084] (2) The weighed high-temperature-resistant masterbatch raw materials are used to blend, modify and granulate PE / PP using PET or PA6 through a parallel twin-screw extruder to obtain a high-temperature-resistant masterbatch, specifically using the following process:

[0085] PET+LLDPE+PP+GMA-g-PE+antioxidant masterbatch——weightless metering, mixing and stirring——parallel twin-screw granulator——granulation——drying——inspection——packaging.

[0086] Among them, granulation temperature (℃): 160, 200, 250, 260, 270, 270, 270, 260, 250.

[0087] Melt temperature (℃): 250. Melt pressure: 4-6Mpa, rotation speed: 300-400r / min.

[0088] (3) Using a three-layer film blowing machine, the high temperature resistant masterbatch is mixed with the PE raw material in proportion and placed in the middle layer of the film blowing, and a three-layer film blowing is performed to obtain the following Figure 1 The high temperature resistant substrate layer shown;

[0089] The film blowing process is: metering of each layer - extrusion by extruder - blowing by die head - traction and stretching - corona - edge cutting - film sheet winding - rewinding and slitting according to customer requirements.

[0090] Specifically, the surface layer is a silicon-coated layer made by extruding a blend of HDPE+LLDPE; the middle layer is a high-temperature resistant layer made by blending high-temperature resistant masterbatch+HDPE, which mainly plays the role of high-temperature resistance and cost reduction; the bottom layer is a color layer made by extruding a blend of HDPE+LLDPE+masterbatch.

[0091]

[0092]

[0093] Process: Film blowing temperature

[0094]

[0095] Among them, screw speed: 60 ~ 100r / min; melt pressure: 35 ~ 50mpa; line speed: 20 ~ 40m / min.

[0096] (II) Preparation of oil-resistant coating

[0097] (1) Weigh 45 parts of vinylidene chloride, 10 parts of sodium methacrylate, 5 parts of butyl acrylate, 5 parts of acrylic acid, 2 parts of methyl methacrylate, 1 part of azobisisobutyronitrile, 1.5 parts of polyoxyethylene ether, 0.6 parts of dimethyl silicone oil, and 29.9 parts of water according to the formula ratio;

[0098] (2) Add all of the vinylidene chloride, sodium methacrylate sulfonate, 1 / 3 of azobisisobutyronitrile, 1 / 3 of polyoxyethylene ether and 3 / 4 of water into a reaction kettle, heat the reaction kettle to 65° C., and stir at 450 r / min for 12 min to obtain a mixed solution A;

[0099] (3) then continuously and uniformly adding all of the butyl acrylate, acrylic acid, methyl methacrylate and the remaining water into the reaction kettle slowly within one hour, and continuing stirring for 1.5 hours to obtain a mixed solution B;

[0100] (4) adding the remaining polyoxyethylene ether of azobisisobutyronitrile and all the polyoxyethylene ether and dimethyl silicone oil to the reactor in sequence, raising the temperature to 75° C., and stirring at 300 r / min for 18 min to obtain a PVDC emulsion;

[0101] (5) A PVDC coating is applied on the surface of the high temperature resistant substrate layer by a coating machine, and the moisture is dried at 105° C. to obtain an oil-resistant coating on the surface of the high temperature resistant substrate layer.

[0102] (III) Preparation of silicone oil release layer

[0103] Continue to use the coating machine to apply silicone oil on the surface of the oil-resistant coating. The silicone oil material is a heat-curing vinyl addition reaction silicone oil, and solidify at 140-150°C and cool to obtain Figure 3 The high-adhesion and high-temperature resistant PE release film shown has a surface layer of a silicone oil release layer, an intermediate layer of an oil-resistant coating, and a bottom layer of a high-temperature substrate layer; then the high-adhesion and high-temperature resistant PE release film prepared above is inspected and rolled up.

[0104] Among them, in the high-adhesion and high-temperature resistant PE release film, the thickness of the oil-resistant coating is 0.0003-0.001 mm, the thickness of the high-temperature substrate layer is 0.025-0.04 mm, and the thickness of the silicone oil release layer is 0.0003-0.0006 mm. The high-adhesion and high-temperature resistant PE release film is marked as S1.

[0105] Example 2 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0106] Different from the above-mentioned Example 1, the high temperature resistant masterbatch in step (i) adopts the following raw material components: 25 parts of PET, 30 parts of PP, 25 parts of LLDPE, 5 parts of GMA-g-PE, and 1 part of antioxidant masterbatch.

[0107] In the multi-layer film blowing process, the three-layer film blowing machine is also used, and the film blowing process is the same. The difference is that according to the temperature resistance requirements, the proportion of the middle layer is adjusted, and the proportion of high temperature resistant masterbatch is 70% and HDPE 30%.

[0108] The preparation of other oil-resistant coatings and silicone oil release layers is the same as that in Example 1. The prepared high-adhesion and high-temperature resistant PE release film is marked as S2.

[0109] Example 3 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0110] Different from the above-mentioned Example 1, the high temperature resistant masterbatch in step (i) adopts the following raw material components: 35 parts of PA6, 30 parts of HDPE, 25 parts of LLDPE, 7 parts of GMA-g-PE, and 2 parts of antioxidant masterbatch.

[0111] In the multi-layer film blowing process, the three-layer film blowing machine is also used, and the film blowing process is the same. The difference is that according to the temperature resistance requirements, the proportion of the middle layer is adjusted, and the proportion of high temperature resistant masterbatch is 70% and HDPE 30%.

[0112] The preparation of other oil-resistant coatings and silicone oil release layers is the same as in Example 1. The prepared high-adhesion and high-temperature resistant PE release film is marked as S3.

[0113] Example 4 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0114] (I) Preparation of high temperature resistant substrate layer

[0115] (1) Weigh the raw material components of high temperature resistant masterbatch respectively by weight: 30 parts of PET, 35 parts of PP or HDPE, 20 parts of LLDPE, 6 parts of GMA-g-PE, and 1.5 parts of antioxidant masterbatch;

[0116] (2) The weighed high-temperature-resistant masterbatch raw materials are used to blend, modify and granulate PE / PP using PET or PA6 through a parallel twin-screw extruder to obtain a high-temperature-resistant masterbatch, specifically using the following process:

[0117] PET+LLDPE+PP+GMA-g-PE+antioxidant masterbatch——weightless metering, mixing and stirring——parallel twin-screw granulator——granulation——drying——inspection——packaging.

[0118] Among them, granulation temperature (℃): 160, 200, 250, 260, 270, 270, 270, 260, 250.

[0119] Melt temperature (℃): 250. Melt pressure: 4-6Mpa, rotation speed: 300-400r / min.

[0120] (3) Using a five-layer film blowing machine, the high temperature resistant masterbatch is mixed with the PE raw material in proportion and placed in the middle layer of the film blowing, and five layers of film blowing are performed to obtain the following Figure 2 The high temperature resistant substrate layer shown;

[0121] The film blowing process is: metering of each layer - extrusion by extruder - blowing by die head - traction and stretching - corona - edge cutting - film sheet winding - rewinding and slitting according to customer requirements.

[0122] Specifically, the surface layer is a silicon-coated layer made by extruding a blend of HDPE+LLDPE; the middle layer is a high-temperature resistant layer made by blending high-temperature resistant masterbatch+HDPE, which mainly plays the role of high-temperature resistance and cost reduction; the bottom layer is a color layer made by extruding a blend of HDPE+LLDPE+masterbatch.

[0123]

[0124] Process: Film blowing temperature

[0125]

[0126] Among them, screw speed: 60 ~ 100r / min; melt pressure: 35 ~ 50mpa; line speed: 20 ~ 40m / min.

[0127] (II) Preparation of oil-resistant coating

[0128] (1) Weigh 45 parts of vinylidene chloride, 10 parts of sodium methacrylate, 5 parts of butyl acrylate, 5 parts of acrylic acid, 2 parts of methyl methacrylate, 1 part of azobisisobutyronitrile, 1.5 parts of polyoxyethylene ether, 0.6 parts of dimethyl silicone oil, and 29.9 parts of water according to the formula ratio;

[0129] (2) Add all of the vinylidene chloride, sodium methacrylate sulfonate, 1 / 3 of azobisisobutyronitrile, 1 / 3 of polyoxyethylene ether and 3 / 4 of water into a reaction kettle, heat the reaction kettle to 65° C., and stir at 450 r / min for 12 min to obtain a mixed solution A;

[0130] (3) then continuously and uniformly adding all of the butyl acrylate, acrylic acid, methyl methacrylate and the remaining water into the reaction kettle slowly within one hour, and continuing stirring for 1.5 hours to obtain a mixed solution B;

[0131] (4) adding the remaining polyoxyethylene ether of azobisisobutyronitrile and all the polyoxyethylene ether and dimethyl silicone oil to the reactor in sequence, raising the temperature to 75° C., and stirring at 300 r / min for 18 min to obtain a PVDC emulsion;

[0132] (5) A PVDC coating is applied on the surface of the high temperature resistant substrate layer by a coating machine, and the moisture is dried at 105° C. to obtain an oil-resistant coating on the surface of the high temperature resistant substrate layer.

[0133] (III) Preparation of silicone oil release layer

[0134] Continue to use the coating machine to apply silicone oil on the surface of the oil-resistant coating. The silicone oil material is a heat-curing vinyl addition reaction silicone oil, which is cured at 140-150°C and cooled to obtain Figure 3 The high-adhesion and high-temperature resistant PE release film shown has a surface layer of a silicone oil release layer, an intermediate layer of an oil-resistant coating, and a bottom layer of a high-temperature substrate layer; then the high-adhesion and high-temperature resistant PE release film prepared above is inspected and rolled up.

[0135] Among them, in the high-adhesion and high-temperature resistant PE release film, the thickness of the oil-resistant coating is 0.0003-0.001 mm, the thickness of the high-temperature substrate layer is 0.025-0.04 mm, and the thickness of the silicone oil release layer is 0.0003-0.0006 mm. The high-adhesion and high-temperature resistant PE release film is marked as S4.

[0136] Example 5 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0137] Different from the above-mentioned Example 4, the high temperature resistant masterbatch in step (i) adopts the following raw material components: 25 parts of PET, 35 parts of HDPE, 28 parts of metallocene (M-LLDPE), 8 parts of GMA-g-PE, and 1.2 parts of antioxidant masterbatch.

[0138] In the multi-layer film blowing process, the three-layer film blowing machine is also used, and the film blowing process is the same. The difference is that according to the temperature resistance requirements, the proportion of the middle layer is adjusted, and the proportion of high temperature resistant masterbatch is 70% and HDPE 30%.

[0139] The preparation of other oil-resistant coatings and silicone oil release layers is the same as that of Example 4. The prepared high-adhesion and high-temperature resistant PE release film is marked as S5.

[0140] Example 6 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0141] Different from the above-mentioned Example 4, the high temperature resistant masterbatch in step (i) adopts the following raw material components: 40 parts of PE, 38 parts of PP, 26 parts of LLDPE, 10 parts of GMA-g-PE, and 1.8 parts of antioxidant masterbatch.

[0142] In the multi-layer film blowing process, the three-layer film blowing machine is also used, and the film blowing process is the same. The difference is that according to the temperature resistance requirements, the proportion of the middle layer is adjusted, and the proportion of high temperature resistant masterbatch is 70% and HDPE 30%.

[0143] The preparation of other oil-resistant coatings and silicone oil release layers is the same as that of Example 4. The prepared high-adhesion and high-temperature resistant PE release film is marked as S6.

[0144] Example 7 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0145] (I) Preparation of high temperature resistant substrate layer

[0146] (1) Weigh the raw material components of high temperature resistant masterbatch by weight: 40 parts of PA6, 40 parts of HDPE, 28 parts of LLDPE, 6 parts of MAH-g-PE, and 2 parts of antioxidant masterbatch;

[0147] (2) The weighed high-temperature-resistant masterbatch raw materials are used to blend, modify and granulate PE / PP using PET or PA6 through a parallel twin-screw extruder to obtain a high-temperature-resistant masterbatch, specifically using the following process:

[0148] PET+LLDPE+PP+GMA-g-PE+antioxidant masterbatch——weightless metering, mixing and stirring——parallel twin-screw granulator——granulation——drying——inspection——packaging.

[0149] Among them, granulation temperature (℃): 160, 200, 250, 260, 270, 270, 270, 260, 250.

[0150] Melt temperature (℃): 250. Melt pressure: 4-6Mpa, rotation speed: 300-400r / min.

[0151] (3) Using a three-layer film blowing machine, the high temperature resistant masterbatch is mixed with the PE raw material in proportion and placed in the middle layer of the film blowing, and a three-layer film blowing is performed to obtain the following Figure 3 The high temperature resistant substrate layer shown;

[0152] The film blowing process is: metering of each layer - extrusion by extruder - blowing by die head - traction and stretching - corona - edge cutting - film sheet winding - rewinding and slitting according to customer requirements.

[0153] Specifically, the surface layer is a silicon-coated layer made by extruding a blend of HDPE+LLDPE; the middle layer is a high-temperature resistant layer made by blending high-temperature resistant masterbatch+HDPE, which mainly plays the role of high-temperature resistance and cost reduction; the bottom layer is a color layer made by extruding a blend of HDPE+LLDPE+masterbatch.

[0154]

[0155]

[0156] Process: Film blowing temperature

[0157]

[0158] Among them, screw speed: 60 ~ 100r / min; melt pressure: 35 ~ 50mpa; line speed: 20 ~ 40m / min.

[0159] (II) Preparation of oil-resistant coating

[0160] (1) Weigh 50 parts of vinylidene chloride, 11 parts of sodium methacrylate, 3 parts of butyl acrylate, 3 parts of acrylic acid, 2 parts of methyl methacrylate, 1 part of azobisisobutyronitrile, 1 part of polyoxyethylene ether, 0.7 parts of dimethyl silicone oil, and 28.3 parts of water according to the formula ratio;

[0161] (2) Add all the vinylidene chloride, sodium methacrylate sulfonate, 1 / 3 of azobisisobutyronitrile, 1 / 3 of polyoxyethylene ether and 3 / 4 of water into a reaction kettle, heat the reaction kettle to 65° C., and stir at 500 r / min for 12 min to obtain a mixed solution A;

[0162] (3) then continuously and uniformly adding all of the butyl acrylate, acrylic acid, methyl methacrylate and the remaining water into the reaction kettle slowly within one hour, and continuing stirring for 2 hours to obtain a mixed solution B;

[0163] (4) Then, the remaining polyoxyethylene ether of azobisisobutyronitrile, all the polyoxyethylene ether and dimethyl silicone oil were added to the reaction kettle in sequence, the temperature was raised to 76° C., and stirred at 300 / min for 16 min to obtain a PVDC emulsion.

[0164] (5) A PVDC coating is applied on the surface of the high temperature resistant substrate layer by a coating machine, and the moisture is dried at 105° C. to obtain an oil-resistant coating on the surface of the high temperature resistant substrate layer.

[0165] (III) Preparation of silicone oil release layer

[0166] Continue to use the coating machine to apply silicone oil on the surface of the oil-resistant coating. The silicone oil material is a thermosetting vinyl addition reaction silicone oil, which is cured at 140-150°C and cooled to obtain a high-adhesion and high-temperature resistant PE release film with a surface layer of a silicone oil release layer, a middle layer of an oil-resistant coating, and a bottom layer of a high-temperature substrate layer; then inspect and roll up the high-adhesion and high-temperature resistant PE release film obtained above.

[0167] Among them, in the high-adhesion and high-temperature resistant PE release film, the thickness of the oil-resistant coating is 0.0003-0.001 mm, the thickness of the high-temperature substrate layer is 0.025-0.04 mm, and the thickness of the silicone oil release layer is 0.0003-0.0006 mm. The high-adhesion and high-temperature resistant PE release film is marked as S7.

[0168] Example 8 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0169] Different from the above-mentioned Example 7, the high temperature resistant masterbatch in step (i) adopts the following raw material components: 35 parts of PA6, 35 parts of PP, 28 parts of LLDPE, 10 parts of MAH-g-PE, and 1.2 parts of antioxidant masterbatch.

[0170] In the multi-layer film blowing process, the three-layer film blowing machine is also used, and the film blowing process is the same. The difference is that according to the temperature resistance requirements, the proportion of the middle layer is adjusted, and the proportion of high temperature resistant masterbatch is 70% and HDPE 30%.

[0171] The preparation of other oil-resistant coatings and silicone oil release layers was the same as in Example 7. The prepared high-adhesion and high-temperature resistant PE release film was marked as S8.

[0172] Example 9 Preparation of high-adhesion and high-temperature resistant PE release film for building waterproof membrane

[0173] Different from the above-mentioned Example 7, the high temperature resistant masterbatch in step (i) adopts the following raw material components: 36 parts of PET, 35 parts of PP, 28 parts of LLDPE, 8 parts of GMA-g-PE, and 1.2 parts of antioxidant masterbatch.

[0174] In the multi-layer film blowing process, the three-layer film blowing machine is also used, and the film blowing process is the same. The difference is that according to the temperature resistance requirements, the proportion of the middle layer is adjusted, and the proportion of high temperature resistant masterbatch is 70% and HDPE 30%.

[0175] The preparation of other oil-resistant coatings and silicone oil release layers was the same as in Example 7. The prepared high-adhesion and high-temperature resistant PE release film was marked as S9.

[0176] Performance Testing

[0177] The conventional common anti-adhesion film was used as the control group, and the high-adhesion and high-temperature resistant PE release films manufactured in the above-mentioned Examples 1 to 9 were used as the experimental group.

[0178] In order to more clearly compare the performance differences between high-adhesion and high-temperature-resistant anti-adhesive films and ordinary anti-adhesive films, the peel strength between coils, the peel strength between coils and aluminum plates, the peel strength between heat-aged coils and coils (non-standard), and the peel strength between heat-aged coils and aluminum plates were specifically tested. The results are shown in the following table:

[0179]

[0180] In summary, the high-adhesion and high-temperature-resistant PE anti-adhesion film manufactured by the coating + material improvement method of the present invention has an adhesion effect increased from ≤50% in the past to >80%, which is twice that of ordinary anti-adhesion films. In addition, the processing performance of the blown film is better, the temperature resistance is also significantly improved, the production cost is reduced by >20%, and the product has a high cost performance.

[0181] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A method for manufacturing a high-adhesion and high-temperature resistant PE release film for building waterproofing membrane, characterized in that: The steps include: (1) Preparation of high temperature resistant substrate layer Weigh the raw material components of the high-temperature-resistant masterbatch, use PET and / or PA6 to blend and modify PE and / or PP through a parallel twin-screw extruder to obtain the high-temperature-resistant masterbatch; use a three-layer or more film blowing machine to blend the high-temperature-resistant masterbatch with the PE raw material in proportion and place it in the middle layer of the film blowing, and perform multi-layer film blowing to obtain a high-temperature-resistant substrate layer; (2) Preparation of oil-resistant coating A coating machine is used to coat PVDC or PVA coating on the surface of the high temperature resistant substrate layer, and the water is dried at 100-150°C to obtain an oil-resistant coating on the surface of the high temperature resistant substrate layer; (3) Preparation of silicone oil release layer Continue to use the coating machine to apply silicone oil on the surface of the oil-resistant coating, solidify at 140-150°C, and cool to obtain a high-adhesion and high-temperature resistant PE release film with a surface layer of silicone oil release layer, a middle layer of oil-resistant coating, and a bottom layer of high-temperature substrate layer; The high temperature resistant masterbatch comprises the following components: PET and / or PA625~40 parts PP and / or HDPE 30~40 parts LLDPE and / or M-LLDPE 15~30 parts Compatibilizer 5~10 parts; The compatibilizer is at least one of MAH-g-PE (maleic anhydride grafted PE) or GMA-g-PE (glycidyl methacrylate grafted PE).

2. The manufacturing method according to claim 1, characterized in that: The PET and / or PA6 are PET; the PP and / or HDPE are PP.

3. The manufacturing method according to claim 1, characterized in that: The LLDPE and / or M-LLDPE is made of LLDPE, and the LLDPE melt index is 1-4 / 10min.

4. The manufacturing method according to claim 1, characterized in that: The high temperature resistant masterbatch comprises the following components in parts by weight: PET25~30 copies PP30~35 LLDPE15~20 parts GMA-g-PE 5~10 parts.

5. The manufacturing method according to any one of claims 2 to 4, characterized in that: The high temperature resistant masterbatch also includes an antioxidant masterbatch, which is formed by mixing and granulating an antioxidant and a LLDPE resin; Among them, the weight of antioxidant in the high temperature resistant masterbatch accounts for 25-35% of the total; The antioxidant is composed of a primary antioxidant 1010 and an auxiliary antioxidant 168 in a weight ratio of 1:

2.

6. The manufacturing method according to claim 1, characterized in that: In the step (2), the oil-resistant coating is a PVDC coating, which is formed by coating a self-adhesive PVDC emulsion prepared from the following components: 40-50 parts of vinylidene chloride, 9-11 parts of sodium methacrylate sulfonate, 3-5 parts of butyl acrylate, 3-5 parts of acrylic acid, 1-2 parts of methyl methacrylate, 0.8-1.4 parts of azobisisobutyronitrile, 1-1.5 parts of polyoxyethylene ether, 0.6-0.8 parts of dimethyl silicone oil, and 23.3-32.5 parts of water.

7. A high-adhesion and high-temperature resistant PE release film for building waterproofing membrane manufactured by the method according to any one of claims 1 to 6, characterized in that: include: A silicone release layer on the surface, an oil-resistant coating in the middle, and a high-temperature substrate layer at the bottom; Wherein, the oil-resistant coating is a PVDC or PVA coating; The high temperature substrate layer is a high temperature resistant multi-layer co-extruded film.

8. The high-adhesion and high-temperature-resistant PE release film for building waterproofing membrane according to claim 7, characterized in that: The high temperature resistant multi-layer co-extruded film comprises: a silicon coating layer located on the surface layer, at least one high temperature resistant layer located in the middle layer, and a color layer located in the bottom layer; Among them, the high temperature resistant layer of the middle layer is composed of a high temperature resistant masterbatch and a PE raw material, the mass fraction of the high temperature resistant masterbatch is 50-80%, and the mass fraction of the PE raw material is 20-50%.

Citation Information

Patent Citations

  • PET release film and manufacturing method thereof

    CN109096513A

  • Release film and manufacturing mathod of the same

    KR101924447B1