A flame retardant composition and preparation method thereof
By adding cellulose hydroxyethyl ether and 3-phosphorylbenzoic acid to the aerogel flame retardant composition, the ignition prevention performance is improved, the problem of poor ignition prevention effect in the prior art is solved, and the further development is achieved Highly efficient flame retardant effect.
Patent Information
- Application Number
- CN202211596956.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The ignition prevention effect of the existing aerogel flame retardant composition is not ideal, and it is necessary to improve the ignition prevention performance.
The flame retardant composition including polyethyleneimine modified silica aerogel, silica sol, cellulose hydroxyethyl ether and 3-phosphorylbenzoic acid is formed by a specific preparation method and proportion combination. Compositions with higher anti-ignition effect.
The ignition prevention effect of the flame retardant composition is significantly improved and has better performance than the prior art.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flame retardancy; specifically, it relates to a flame retardant composition and a preparation method thereof. Background Art
[0002] Aerogel has low thermal conductivity, high specific surface area, high porosity, low density and low refractive index. These physical properties determine the application of silica aerogel in thermal insulation. Silica aerogel has extremely low thermal conductivity, and its spatial network structure is mainly composed of Si-O-Si bonds, so it has good flame retardant properties.
[0003] Xi Yuqin in “Nano-SiO 2 In the article "Flow Characteristics and Effects of Water Mist Fire Extinguishing Agent after Viscosity Modification" (Chemical Industry Progress, 2009, 28, P199), 60-70% nano-SiO 2 The adhesive fire extinguishing agent is prepared with a thickener composed of 25% polyvinyl alcohol and 5% silicone oil. Under similar flow rates, the fire extinguishing time of the adhesive fire extinguishing agent is about a quarter of that of water extinguishing.
[0004] Chinese patent application CN111840880A discloses an aerogel fire extinguishing agent, comprising modified silica aerogel and silica sol; prepared by the following method: adding silica aerogel to a polyethyleneimine aqueous solution with a pH of 5 and dispersing it uniformly to obtain a modified silica aerogel solution; successively adding silica sol and cellulose hydroxyethyl ether and dispersing them uniformly. The fire extinguishing agent has a higher fire extinguishing efficiency and has a certain ignition prevention effect.
[0005] However, the ignition prevention effect of the above-mentioned aerogel flame retardant composition is still unsatisfactory. Summary of the invention
[0006] In view of the above problems, the present invention aims to provide a flame retardant composition with better ignition prevention effect and a preparation method thereof.
[0007] To achieve the above object, on the one hand, the present invention adopts the following technical scheme: a flame retardant composition, comprising:
[0008] Polyethyleneimine-modified silica aerogel;
[0009] Silica sol;
[0010] Cellulose hydroxyethyl ether;
[0011] 3-phosphobenzoic acid;
[0012] water.
[0013] According to the flame retardant composition of the present invention, the sum of the contents of 3-phosphorylbenzoic acid and cellulose hydroxyethyl ether is 1-3 wt %.
[0014] According to the flame retardant composition of the present invention, the content ratio of 3-phosphorylbenzoic acid to cellulose hydroxyethyl ether is (50-70): (30-50).
[0015] According to the flame retardant composition of the present invention, the polyethyleneimine-modified silica aerogel is obtained by adding silica aerogel to a polyethyleneimine aqueous solution with a pH of 5 and dispersing the silica aerogel uniformly; the polyethyleneimine has a number average molecular weight Mn of 1800; an amine value of 19 mmol / g; a primary amine content of 35 mol%; a secondary amine content of 35 mol%; a tertiary amine content of 30 mol%; and a weight ratio of the polyethyleneimine to the silica aerogel of 1:(8-12).
[0016] According to the flame retardant composition of the present invention, the average pore size of the silica aerogel is 28 nm and the density is 0.043 g / cm 3 ;The thermal conductivity is 0.018W / (mK).
[0017] According to the flame retardant composition of the present invention, the content of the modified silica aerogel is 4-8wt%, which is calculated based on the ratio of the sum of the dry matter mass of the silica aerogel and the polyethyleneimine to the mass of the flame retardant composition.
[0018] According to the flame retardant composition of the present invention, the preparation method of the silica aerogel is as follows: a sodium silicate solution is adjusted to pH ≥ 9 by dripping a 2M sulfuric acid solution until a gel phenomenon occurs, and aged at 55°C for 24h; washed with water three times, and then placed in anhydrous ethanol for solvent replacement, wherein the mass ratio of anhydrous ethanol to sodium silicate is 5:1; filtered, dried at normal pressure, dried at a programmed temperature, and finally naturally cooled to obtain; the programmed temperature is 80°C / 2h+100°C / 2h+120°C / 2h; the heating rate is 2°C / min; SiO 2 The content is 10-30wt%.
[0019] According to the flame retardant composition of the present invention, the content of the silica sol is 10-20wt%, which is calculated based on the ratio of the mass of the silica sol to the mass of the flame retardant composition.
[0020] According to the flame retardant composition of the present invention, the content of the cellulose hydroxyethyl ether is 0.5-2wt%; and the viscosity of a 2% aqueous solution of the cellulose hydroxyethyl ether at 20° C. is 2600-3300 mPa.s.
[0021] On the other hand, the present invention also provides a method for preparing the flame retardant composition, comprising:
[0022] The silica sol, cellulose hydroxyethyl ether and 3-phosphorylbenzoic acid, as well as the balance of water, are added successively to the modified silica aerogel dispersion, and the flame retardant composition is obtained after being evenly dispersed.
[0023] Compared with the prior art, the ignition prevention effect of the present invention is further improved. DETAILED DESCRIPTION
[0024] The following examples are intended only to provide a person of ordinary skill in the art with a complete disclosure and description of how to make and evaluate the compounds, compositions, articles, devices and / or methods described and claimed herein, and are intended to be exemplary only and not intended to limit the scope of the inventor's invention. Efforts have been made to ensure accuracy with respect to numbers (e.g., amounts, temperatures, etc.), but some errors and deviations should be taken into account.
[0025] Unless otherwise indicated, parts are by weight, and the parts by weight are calculated based on the total weight of the flame retardant composition. The calculation basis of the sol content includes colloid and water. The temperature is expressed in ° C or at ambient temperature, and the pressure is atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, required solvents, solvent mixtures, temperatures, pressures and other reaction ranges) and conditions that can be used to optimize the product purity and yield obtained by the method. Only reasonable routine experiments will be required to optimize such method conditions.
[0026] Preparation of silica aerogel
[0027] The sodium silicate solution was adjusted to pH ≥ 9 by dropping 2M sulfuric acid solution until gelation occurred, and then aged at 55°C for 24 hours; washed with water three times, and then placed in anhydrous ethanol for solvent replacement, with the mass ratio of anhydrous ethanol to sodium silicate being 5:1; filtered, dried at normal pressure, dried at programmed temperature, and finally cooled naturally. The programmed temperature mechanism was 80°C / 2h+100°C / 2h+120°C / 2h; the heating rate was 2°C / min.
[0028] The average pore size of the silica aerogel is 28 nm, the density is 0.043 g / cm3, and the thermal conductivity is 0.018 W / (mK).
[0029] Preparation of Polyethyleneimine Modified Silica Aerogel
[0030] The silica aerogel is added to a polyethyleneimine aqueous solution with a pH of 5 and dispersed uniformly to obtain a modified silica aerogel solution; the polyethyleneimine has a number average molecular weight Mn of 1800; an amine value of 19 mmol / g; a primary amine content of 35 mol%; a secondary amine content of 35 mol%; a tertiary amine content of 30 mol%. The weight ratio of the polyethyleneimine to the silica aerogel is 1:10.
[0031] Example 1
[0032] The flame retardant composition comprises:
[0033] 6 wt% of polyethyleneimine-modified silica aerogel;
[0034] Silica sol (SiO 2 Content is 20wt%);
[0035] 0.8 wt% cellulose hydroxyethyl ether (viscosity of 2% aqueous solution at 20°C is 2600-3300 mPa.s);
[0036] 3-phosphorylbenzoic acid in an amount of 1.2 wt%;
[0037] The balance is water.
[0038] The preparation method of the flame retardant composition is as follows:
[0039] The silica sol, cellulose hydroxyethyl ether and 3-phosphorylbenzoic acid, as well as the balance of water, are added successively to the modified silica aerogel dispersion, and the flame retardant composition is obtained after being evenly dispersed.
[0040] Comparative Example 1
[0041] The flame retardant composition was obtained by using 2 wt % of 3-phosphorylbenzoic acid in total to replace both cellulose hydroxyethyl ether and 3-phosphorylbenzoic acid in Example 1, and other conditions were the same as those in Example 1.
[0042] Flame retardant performance test
[0043] According to the test conditions of Xi Yuqin's article, the flame retardant compositions of Example 1 and Comparative Example 1 were used for testing. The ignition time of the wood strips impregnated with the flame retardant compositions of Example 1 and Comparative Example 1 when in direct contact with the flame was measured (average value was taken). The results are shown in Table 1.
[0044] Table 1
[0045] test Ignition time(s) Example 1 463 Comparative Example 1 372
[0046] It can be seen from Table 1 that, compared with Comparative Example 1, the flame retardant composition of Example 1 of the present invention has a better effect of preventing ignition.
[0047] It should be understood that the specific embodiments of the present invention are only used to illustrate the spirit and principles of the present invention, and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes, substitutions, deletions, corrections or adjustments to the technical solutions of the present invention, and these equivalent technical solutions also fall within the scope defined by the claims of the present invention.
Claims
1. A flame retardant composition, characterized in that: include: Polyethyleneimine-modified silica aerogel; Silica sol; Cellulose hydroxyethyl ether; 3-phosphobenzoic acid; water; in, The content of the modified silica aerogel is 4-8wt%, which is calculated based on the ratio of the sum of the dry matter mass of the silica aerogel and the polyethyleneimine to the mass of the flame retardant composition; The polyethyleneimine-modified silica aerogel is obtained by adding silica aerogel to a polyethyleneimine aqueous solution with a pH of 5 and uniformly dispersing the silica aerogel; the polyethyleneimine has a number average molecular weight Mn of 1800; an amine value of 19 mmol / g; a primary amine content of 35 mol%; a secondary amine content of 35 mol%; a tertiary amine content of 30 mol%; and a weight ratio of the polyethyleneimine to the silica aerogel of 1:(8-12); The content of the silica sol is 10-20wt%; calculated based on the ratio of the mass of the silica sol to the mass of the flame retardant composition; The sum of the contents of 3-phosphorylbenzoic acid and cellulose hydroxyethyl ether is 1-3wt%; the content ratio of 3-phosphorylbenzoic acid to cellulose hydroxyethyl ether is (50-70): (30-50); The average pore size of the silica aerogel is 28 nm and the density is 0.043 g / cm 3 ;Thermal conductivity is 0.018W / (mK); The content of the cellulose hydroxyethyl ether is 0.5-2wt%; the viscosity of a 2% aqueous solution of the cellulose hydroxyethyl ether at 20°C is 2600-3300mpa.s.
2. The flame retardant composition according to claim 1, wherein The preparation method of the silica aerogel is as follows: adjusting the pH of the sodium silicate solution to ≥9 by dropping a 2M sulfuric acid solution until gelation occurs, and aging at 55°C for 24h; washing with water three times, and then placing in anhydrous ethanol for solvent replacement, wherein the mass ratio of anhydrous ethanol to sodium silicate is 5:1; drying at normal pressure after suction filtration, drying at a programmed temperature, and finally cooling naturally; the programmed temperature is 80°C / 2h+100°C / 2h+120°C / 2h; the heating rate is 2°C / min; the SiO2 content in the silica sol is 10-30wt%.
3. A method for preparing the flame retardant composition according to claim 1 or 2, comprising: The silica sol, cellulose hydroxyethyl ether and 3-phosphorylbenzoic acid, as well as the balance of water, are added successively to the modified silica aerogel dispersion, and the flame retardant composition is obtained after being evenly dispersed.