A kind of CH1T ultra-low carbon cold heading steel and its preparation method
By adding slag washing materials and aluminum particles during the converter smelting and LF refining processes, and controlling the Al2O3 content and argon gas input, the problem of low desulfurization rate when the temperature of the molten iron is low is solved, and the desulfurization efficiency and quality of cold heading steel are improved. .
Patent Information
- Application Number
- CN202310083763.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-08
AI Technical Summary
In the existing technology, when the temperature of the molten iron is lower than 1350°C, the desulfurization rate of the molten iron pretreatment is low, resulting in poor desulfurization effect of cold heading steel CH1T and affecting its quality.
During the process of converter smelting and LF refining, slag washing materials and aluminum particles are added for converter tapping alloying. The Al2O3 content in the slag is controlled to 25% to 30%. When the temperature of the molten steel reaches 1600℃±10℃, strong stirring is started. Desulfurization, and optimize the desulfurization effect by adjusting the slag viscosity and argon gas input.
It improves the desulfurization efficiency and quality, ensures the finished product quality of CH1T ultra-low carbon cold heading steel, and solves the problems of poor slag fluidity and difficult desulfurization.
Smart Images

Figure BDA0004068358730000121 
Figure BDA0004068358730000131 
Figure BDA0004068358730000132
Abstract
Description
Technical Field
[0001] The present invention relates to the field of smelting technology, and in particular to a CH1T ultra-low carbon cold heading steel and a preparation method thereof. Background Art
[0002] CH1T belongs to the ultra-low carbon pure iron series steel. The product has the advantages of low harmful elements, high steel purity, high geometric dimensional accuracy, good electromagnetic performance, soft material, and excellent toughness. It has complex process conditions and is mainly used for deep drawing. It is widely used in the manufacture of hollow rivets for automobiles, engineering machinery and toys, hollow rivets for luggage, stamping parts, forging parts, special-shaped parts with large deformation, and electronic components such as electromagnetic valve gaskets.
[0003] The production process flow of cold heading steel CH1T provided by relevant technology: blast furnace molten iron → (mixed iron furnace) → molten iron desulfurization pretreatment → 120t converter smelting → LF refining → RH refining → small square billet continuous casting machine continuous casting → billet stack cooling → billet inspection and cleaning → billet cold charging heating furnace heating → smelting and rolling mill → high-speed wire controlled rolling and controlled cooling → finishing → inspection → packaging → weighing → warehousing.
[0004] The desulfurization effect will directly affect the quality of cold heading steel CH1T. Generally speaking, desulfurization is carried out by hot metal pretreatment and LF dual desulfurization. However, when the hot metal temperature is less than 1350℃, the desulfurization rate of hot metal pretreatment is low, and the S content of hot metal entering the furnace is greater than 0.010%. The slag system used in LF is difficult to dilute the CaS concentration, which is not conducive to the desulfurization effect, making it difficult to improve the desulfurization effect of cold heading steel CH1T, affecting the quality of cold heading steel CH1T.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a CH1T ultra-low carbon cold heading steel with high desulfurization efficiency and good effect and a preparation method thereof, which can effectively ensure the quality of the CH1T ultra-low carbon cold heading steel.
[0007] The embodiment of the present invention is achieved as follows:
[0008] In a first aspect, the present invention provides a method for preparing CH1T ultra-low carbon cold heading steel, comprising converter smelting, LF refining, RH refining and continuous casting performed in sequence;
[0009] Among them, slag washing slag and aluminum particles are added during converter smelting and steel tapping for converter steel tapping alloying and slag washing treatment, and in the LF refining process, when the molten steel temperature reaches the first preset temperature T0, strong stirring is turned on for desulfurization, T0 is 1600℃±10℃, and when strong stirring is turned on, the Al in the slag is controlled. 2 O 3The content is 25% to 30%, and the cross-sectional thickness value d of the slag block on the slag sticking rod is in the range of 1.50-1.55mm.
[0010] In an optional embodiment, when strong stirring is turned on, the argon gas flow rate is 55-65Nm 3 / h, the exposed diameter of molten steel is 50cm to 60cm; preferably, when strong stirring is turned on, the argon gas flow rate is 60 3 / h, the exposed diameter of molten steel is 55cm.
[0011] In an optional embodiment, after the steel is smelted in the converter, the method further comprises taking a sample at an argon station to obtain an argon station [S]% in the molten steel;
[0012] The preparation method also includes determining the strong stirring time according to the argon station [S]% and the specified value 0.010% of the CH1T ultra-low carbon cold heading steel process card when the molten steel temperature reaches the first preset temperature; wherein, when the argon station [S]% is less than 0.010%, the strong stirring time is 5 minutes, and when the argon station [S]% is greater than 0.010%, the strong stirring time S=5+(argon station [S]%-0.010%)÷0.010%×5.
[0013] In an optional embodiment, the slag washing material includes lime akg / ton steel and fluorite bkg / ton steel, a is 6.7-7.2, b is 0.8-1.0; the amount of aluminum particles is ckg / ton steel, c is 1.6-1.8kg / ton steel; and LF refining includes temperature measurement at the station, low-speed electrification slag, adjustment of slag viscosity, and high-speed electrification to a first preset temperature and strong stirring desulfurization;
[0014] Among them, by adding fluorite and lime in the process of adjusting the viscosity of the slag, the cross-sectional thickness value d of the slag block on the slag sticking rod is controlled between 1.50-1.55 mm; and the additional amount of fluorite Wfluorite addition = 0.2×(d1-1.5) kg / ton of steel, the additional amount of lime Wlime addition = 0.6×(d1-1.5) kg / ton of steel, d1 is the real-time measurement value of the cross-sectional thickness of the slag block on the slag sticking rod.
[0015] In an optional embodiment, the heating rate of the low-speed power transmission slag-forming process is V1°C / min, the slag-forming time is t1, and the slag-forming end temperature is T1; the heating rate of the high-speed power transmission process is V2°C / min, and the slag-forming time is t2=(T0-T1) / V2; the argon gas flow rate of the high-speed power transmission and the low-speed power transmission slag-forming is 35-40Nm 3 / h, the exposed diameter of molten steel is 25cm~30cm;
[0016] In the process of high-speed power transmission, aluminum particles are added to make up for the aluminum content lost in the process of low-speed power transmission and high-speed power transmission, so as to control the Al content in the slag. 2 O3 The content is 25% to 30%; among them, the mass of added aluminum particles G1 is determined by the aluminum content △[Als] lost through power transmission and temperature increase and the sulfur content lost during the strong stirring process △[Als]1, G1 aluminum particle addition = △[Als] × 0.01 × 1000kg / ton of steel + △[Als] 1 × 0.01 × 1000kg / ton of steel, △[Als] = (t1+t2) × 0.0015%, △[Als] 1 = S × 0.003%.
[0017] In an optional embodiment, after the strong stirring is completed, sampling is also included to obtain LF1 [Als] % and LF1 [Mn] %;
[0018] After the high-speed power supply is delivered to the first preset temperature and the desulfurization is carried out by strong stirring, the high-speed power supply is continued to be delivered to the second preset temperature T2, T2 is 1675℃±5℃; and in the process of continuing the high-speed power supply, aluminum particles and low-carbon ferromanganese are added to adjust the aluminum content LF2 [Als] % in the molten steel to 0.005%~0.009%, so as to control the manganese content LF2 [Mn] % in the molten steel within the process card target of 0.10%.
[0019] In an optional embodiment, during the high-speed power transmission process, the amount of argon gas introduced is 35-40 Nm 3 / h, the exposed diameter of the molten steel is 25cm~30cm, and the heating rate is V2℃ / min; and the mass of aluminum particles that need to be added is jointly determined according to the Als content lost in the heating process, LF1[Als]%, and LF2[Als]%, G2 aluminum particles addition = (T2-T0) / V2×0.0015%×0.01×1000kg / ton of steel + (LF1[Als]%-(T2-T0) / V2×0.0015%-LF2[Als]%)×0.01×1000kg / ton of steel.
[0020] In an optional embodiment, assuming that all the aluminum particles added with the slag washing material are used to increase the Als content in the molten steel, the Als content of the aluminum particles is c%; after the converter smelts the steel, it also includes sampling at the argon station to obtain the argon station [Als]% in the molten steel, and the argon station [Als]% is controlled between 0.020% and 0.040%;
[0021] Al in slag 2 O 3 The content G furnace is calculated by the argon station [Als]%, c% and the loss of aluminum in the molten steel e%, and G furnace = (c% - argon station [Als]% - e%) × 80%; among them, e% is 0 before the electro-slag is sent, and when the electro-slag is sent to make the molten steel temperature reach the first preset temperature, e% = △ [Als] + △ [Als] 1.
[0022] In an optional embodiment, the LF final slag includes CaO: 52% to 54%, SiO 2 :3%~5%,Al 2 O 3 : 25% to 30%, FeO: 0.7% to 0.8%, MnO: 0.2% to 0.3%, S: 0.3% to 0.5%, MgO: 5% to 7%, P 2 0 5 : 0.05~0.08%, R: 10~18, and W(FeO+MnO) in LF final slag is <1%.
[0023] In a second aspect, the present invention provides a CH1T ultra-low carbon cold heading steel, which is prepared by the preparation method of the CH1T ultra-low carbon cold heading steel of any one of the aforementioned embodiments.
[0024] The embodiments of the present invention have at least the following advantages or beneficial effects:
[0025] The preparation method of CH1T ultra-low carbon cold heading steel provided by the embodiment of the present invention comprises converter smelting, LF refining, RH refining and continuous casting performed in sequence; wherein, when the converter smelts and taps the steel, slag washing slag and aluminum particles are added to perform converter tapping alloying and slag washing treatment, and during the LF refining process, when the molten steel temperature reaches a first preset temperature T0, strong stirring is turned on for desulfurization, T0 is 1600°C±10°C, and when the strong stirring is turned on, the Al in the slag is controlled 2 O 3 The content is 25% to 30%, and the cross-sectional thickness value d of the slag block on the slag sticking rod is in the range of 1.50-1.55mm.
[0026] The preparation method comprises the following steps: 2 O 3 By controlling the content of and the cross-sectional thickness d of the slag block of the sticky slag rod, the fluidity of the slag corresponding to the desulfurization temperature can be adjusted to the optimal level, so that the desulfurization efficiency and quality can be fully improved to ensure the quality of the finished steel.
[0027] The embodiment of the present invention further provides a CH1T ultra-low carbon cold heading steel, which is prepared by the above preparation method. Therefore, it also has the advantage of high quality. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0029] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0030] An embodiment of the present invention provides a CH1T ultra-low carbon cold heading steel, which is prepared by the following preparation method:
[0031] S1: converter smelting;
[0032] The converter is a process of smelting steel and iron together to form molten steel. The converter endpoint C is controlled at 0.04% to 0.05%, the endpoint O is controlled at 400 to 600 ppm, P is controlled at ≤0.010%, and the tapping temperature is controlled at 1640±20℃.
[0033] At the same time, slag washing slag and aluminum particles are added during converter smelting and steel tapping to alloy converter steel tapping and slag washing treatment to ensure the subsequent deoxidation and desulfurization effects to ensure the quality of finished steel. Among them, slag washing slag includes lime akg / ton steel and fluorite bkg / ton steel, a is 6.7~7.2, b is 0.8~1.0; the amount of aluminum particles is ckg / ton steel, c is 1.6~1.8kg / ton steel.
[0034] Generally speaking, the amount of lime added during the washing and alloying of converter slag is 2.5-2.7 kg lime / ton steel, and the amount of aluminum iron is 4.1-4.3 kg aluminum iron / ton steel. In the LF process, slag-making material: 4.2-4.4 kg lime / ton steel is added to assist desulfurization. The problem is that the amount of lime used in the LF slag system is small, and the small amount of slag cannot dilute the CaS concentration in the slag, which is not conducive to the desulfurization effect; and this type of steel does not add fluorite, which makes the Al in the early LF slag 2 O 3 The content is low, the slag fluidity is poor, the slag interface reaction is weak, and the desulfurization of the molten steel is difficult. For this reason, in the embodiment of the present invention, the LF slag-making material is added simultaneously with the alloying slag material when the converter is tapped, and aluminum particles (Al content is 99.7% to 99.9%, and the specification is 6*6mm) are added to replace the aluminum iron with a larger specific gravity (Al content is 40% to 45%, and the specification is 20*20mm.), which is equivalent to diffusion deoxidation of the molten steel instead of precipitation deoxidation of the molten steel, which can ensure the deoxidation and desulfurization efficiency. At the same time, the molten steel alloyed with aluminum deoxidation, in addition to producing the necessary Als, also produces Al 2 O 3 Inclusions. 2 O 3 Most of it can float to the slag under argon gas dynamic conditions, which can improve the fluidity of the slag and further improve the desulfurization efficiency and quality.
[0035] In addition, it should be noted that during the steel tapping process of the converter, 60 Nm of strong stirring argon gas was introduced. 3 / h, the exposed diameter of molten steel is 50cm~60cm (preferably 55cm), so that the slag interface reacts fully, the efficiency of removing O and S is improved, and the yellow-white slag state is initially achieved. After the converter is tapped, the argon flow rate is reduced to 30Nm for weak stirring. 3 / h, the exposed diameter of molten steel is 20cm-30cm (preferably 25cm), further deoxidation and desulfurization, so that Al in the molten steel 2 O 3 Float into the slag to improve the fluidity of the slag.
[0036] S2: LF refining; specifically, the steps of LF refining include:
[0037] S21: Temperature measurement before entering the station; before entering the station, sampling can be done at the argon station, and Als can be controlled at 0.020% to 0.040%, and the argon station [Als]% and argon station [S]% can be obtained for subsequent use. When entering the station, temperature measurement is performed to measure whether the entry temperature meets the requirements.
[0038] S22: low gear to send electrochemical slag;
[0039] The heating rate of the low-speed power transmission slag-forming process is V1℃ / min, the slag-forming time is t1, and the slag-forming end temperature is T1. Among them, in the embodiment of the present invention, the low gear is specifically selected as gear 8, the theoretical heating rate of gear 8 is V1=4℃ / min, and the slag-forming time t1 can be selected as 3min. In other embodiments, it can also be fine-tuned, which is not limited here. At the same time, during the low-speed power transmission slag-forming process, argon gas 35~40Nm 3 / h, the exposed diameter of molten steel is 25cm~30cm, preferably 28cm, to fully ensure the fluidity of slag and to ensure the desulfurization efficiency in the later stage.
[0040] S23: adjusting slag viscosity;
[0041] The purpose of adjusting the viscosity of the slag is to adjust the fluidity of the slag to ensure the desulfurization effect in the later stage. In addition, by adding fluorite and lime in the process of adjusting the viscosity of the slag, the cross-sectional thickness value d of the slag block on the sticky slag rod is controlled between 1.50-1.55mm; when the cross-sectional thickness value d of the slag block of the iron pipe sticky slag increases by 1.5mm, 0.2kg / ton of steel of fluorite balls needs to be added, so that the amount of fluorite added W fluorite added = 0.2×(d1-1.5)kg / ton of steel, the amount of lime added W lime added = 0.6×(d1-1.5)kg / ton of steel, so that W lime added: W fluorite ball added is approximately 3:1. Among them, d1 is the real-time measurement value of the cross-sectional thickness of the slag block on the sticky slag rod, which is measured after 3 minutes of electrification of the slag at low gear. By adding fluorite and lime, the cross-sectional thickness d of the slag block on the slag sticking rod can be controlled between 1.50-1.55mm, so as to fully ensure the fluidity of the slag and ensure the subsequent desulfurization effect.
[0042] S24: high-speed power transmission to the first preset temperature and strong stirring for desulfurization;
[0043] After adjusting the slag viscosity, power can be supplied until the molten steel temperature reaches the first preset temperature T0, T0 is 1600℃±10℃, the heating rate of the high-speed power supply process is V2℃ / min, and the slag melting time is t2=(T0-T1) / V2. For example, the high-speed can be selected as the 2nd gear, at which V2=8℃ / min. The argon gas flow rate for high-speed power supply and low-speed power supply is 35~40Nm 3 / h, the exposed diameter of molten steel is 25cm~30cm. When the temperature meets this requirement, strong stirring is turned on for desulfurization, and when strong stirring is turned on, the Al content in the slag is controlled. 2 O 3 The content of is 25% to 30%, and the cross-sectional thickness value d of the slag block on the slag sticking rod is in the range of 1.50-1.55mm. When the strong stirring is turned on, the argon gas flow rate is 55-65Nm 3 / h, the exposed diameter of molten steel is 50cm to 60cm; preferably, when strong stirring is turned on, the argon gas flow rate is 60 3 / h, the exposed diameter of molten steel is 55cm.
[0044] Since Al in slag 2 O 3 The slag has the best fluidity when the content of Al in the slag is 25% to 30% and the cross-sectional thickness d of the slag block on the slag sticking rod is in the range of 1.50-1.55 mm. 2 O 3 By controlling the content of and the cross-sectional thickness d of the slag block of the sticky slag rod, the fluidity of the slag corresponding to the desulfurization temperature can be adjusted to the optimal level, so that the desulfurization efficiency and quality can be fully improved to ensure the quality of the finished steel.
[0045] It should be noted that in the embodiments of the present invention, Al in the slag 2 O 3 The content is preferably 28%. After the arc temperature reaches the preset requirement of 1600℃, the weight of Al2O3 in the slag G is 28%, and the slag fluidity is optimal; the cross-sectional thickness of the thin white slag d slag sample is 1.5mm, W (FeO + MnO) in the slag is less than 1%, and the Als content is 0.030%. At this time, a strong stirring argon gas of 60Nm is introduced at a relatively high molten steel temperature of 1600℃. 3 / h, the exposed diameter of molten steel is 50cm-60cm (preferably 55cm), so that the steel slag interface reacts fully, the molten steel is deeply desulfurized, and the desulfurization effect is optimal. Strong stirring has a great influence on the slag-steel sulfur distribution ratio LS. After strong stirring for a certain period of time, the slag-steel sulfur distribution ratio reaches saturation, and LS gradually decreases, which can fully ensure the desulfurization quality and efficiency.
[0046] It should also be noted that the time of strong stirring is related to the sulfur content. The higher the sulfur content, the longer the time of strong stirring. Based on this, in an embodiment of the present invention, the preparation method also includes determining the strong stirring time according to the argon station [S]% and the specified value 0.010% of the CH1T ultra-low carbon cold heading steel process card when the molten steel temperature reaches the first preset temperature; wherein, when the argon station [S]% is less than 0.010%, the strong stirring time is 5min, and when the argon station [S]% is greater than 0.010%, the strong stirring time S=5+(argon station [S]%-0.010%)÷0.010%×5. By accurately calculating the strong stirring time, the deoxidation efficiency and quality can be further improved, and the deoxidation time can be saved.
[0047] In addition, as an optional solution, aluminum particles can be added during the high-speed power transmission process to make up for the aluminum content lost during the low-speed power transmission slag and high-speed power transmission process, so as to fully ensure that the Al content in the slag is 2 O 3 The content of argon is 25% to 30%. In production practice, this kind of slag is selected to pass argon gas 35 to 40Nm 3 / h, when the exposed diameter of molten steel is 25cm to 30cm, preferably 28cm, the arc submergence effect is better, and the Als content loses 0.0015% every 1min. At the same time, the strong stirring step in the strong stirring desulfurization process will also lead to the loss of aluminum content, in order to reduce the aluminum content in the molten steel, so that the mass of the added aluminum particles G1 aluminum particles added by the aluminum content △ [Als] lost by power transmission and heating and the sulfur content lost during the strong stirring process is △ [Als] 1 jointly determined, G1 aluminum particles added = △ [Als] × 0.01 × 1000kg / ton of steel + △ [Als] 1 × 0.01 × 1000kg / ton of steel, △ [Als] = (t1 + t2) × 0.0015%, △ [Als] 1 = S × 0.003%. By adding aluminum particles, it can be fully guaranteed that the Al content in the slag 2 O 3 The content is between 25% and 30%, so as to fully ensure the fluidity of the slag, to fully improve the desulfurization efficiency and quality, and to ensure the quality of the finished steel.
[0048] It should be noted that, in this embodiment, in order to ensure that Al 2 O 3 The content of Al in the slag is 25% to 30%. 2 O 3 The content of Al in slag can be accurately calculated. The embodiment of the present invention also provides 2 O 3 The method for calculating the content of aluminum includes: calculating by argon station [Als]%, c% and the loss of aluminum in molten steel e%, and G furnace = (c%-argon station [Als]%-e%) × 80%; wherein, before sending the electroslag, e% is 0, that is, when there is no electroslag, there is no loss, and it can be directly calculated at this time. When the electroslag is sent to make the molten steel temperature reach the first preset temperature, e% = △ [Als], that is, when the electroslag is sent, there is aluminum loss, and it is necessary to recalculate through the loss to ensure that the Al in the slag calculated in each link is 2 O 3 The content is accurate, which can fully guarantee the desulfurization quality and desulfurization efficiency.
[0049] Among them, for example, the normal total weight of slag G is 7.5-8.2 kg / ton steel, preferably 8.2 kg / ton steel. When Al2O3 in the slag is 25%-30%, preferably 28%, the slag fluidity and steel liquid desulfurization effect are the best. 2 O 3 The mass of steel is 2.3 kg / ton steel. Due to the aluminum deoxidation alloying, in addition to the AlS required for the composition, Al 2 O 3 Inclusions. 2 O 3Most of them can float to the slag under argon gas dynamic conditions. 2 O 3 The mass of G slag Al 2 O 3 80% of the total mass of G slag. 2 O 3 The total mass of Al 2 O 3 ÷80%=2.3÷80%=2.9 (kg / ton steel). Therefore, it can be concluded that Al is 1.5kg / ton steel, and Al can be converted to increase the Als content by 0.15%, that is, the Als content in the molten steel is 0.15% and all of it is converted to Al. 2 O 3 When floating to the slag, the Al in the slag 2 O 3 The weight proportion is 28%, which also proves that the embodiment of the present invention can fully meet the subsequent desulfurization and deoxidation requirements by adding 1.7 kg / ton of steel during the converter steel alloying.
[0050] As another example, when the electrified slag is sent to make the molten steel temperature reach the first preset temperature, 1.7 kg of aluminum particles / ton of steel are added to the converter slag. If all of them are used to increase the Als content in the molten steel, the Als content can be increased by 0.17%. At the same time, after the aluminum particles G1 are added, the aluminum particles added = △ [Als] × 0.01 × 1000 kg / ton of steel + △ [Als] 1 × 0.01 × 1000 kg / ton of steel, △ [Als] = (t1 + t2) × 0.0015%, △ [Als] 1 = S × 0.003%, the Al in the slag 2 O 3 Content = (0.17% - argon station [Als]% - △ [Als]% - △ [Als] 1%) × 80%.
[0051] S25: Take samples and continue to supply power at a high level to a second preset temperature.
[0052] After the strong stirring is completed, sampling is also included to obtain LF1 [Als]% and LF1 [Mn]%, so as to facilitate the subsequent adjustment of aluminum content and manganese content. Specifically, it is found in production practice that when the Als content of the molten steel is less than 0.005%, reoxidation and resulfurization will occur, affecting the results of the previous desulfurization. When the Als content of the molten steel is between 0.005% and 0.009%, the resulfurization of the molten steel can be inhibited. However, CH1T ultra-low carbon cold heading steel needs to be decarburized by RH oxygen blowing. Once the Als content of the molten steel is high, the aluminum-oxygen reaction reduces the RH decarburization efficiency, increases the oxygen blowing cost, generates excess temperature, and produces a large amount of Al2O3 inclusions. Therefore, after sampling, in the process of continuing high-speed power transmission, it is necessary to adjust the Als content of the molten steel to between 0.005% and 0.009%, preferably 0.006%.
[0053] In detail, after the high-speed power transmission reaches the first preset temperature and the strong stirring desulfurization is carried out, the high-speed power transmission is continued to the second preset temperature T2, T2 is 1675℃±5℃, the gear is still the 2nd gear, and the heating rate is 8℃ / min. 35~40Nm of argon is introduced 3 / h, the exposed diameter of the molten steel is 25cm-30cm, preferably 28cm. In the process of continuing high-speed power transmission, aluminum particles and low-carbon ferromanganese are added to adjust the aluminum content LF2 [Als]% in the molten steel to 0.005%-0.009%, preferably 0.006%, and the manganese content LF2 [Mn]% in the molten steel is controlled within the process card target of 0.10%.
[0054] In addition, since the high-speed power transmission leads to a loss of aluminum content, it is necessary to add aluminum particles again according to the aforementioned replenishment mechanism during this process, with argon gas 35-40Nm 3 / h, when the exposed diameter of molten steel is 25cm-30cm, preferably 28cm, the arc submergence effect is better, and the Als content loses 0.0015% every 1min. Therefore, the mass of aluminum particles to be added is determined based on the Als content lost during the heating process, LF1 [Als]%, and LF2 [Als]% G2 aluminum particles added = (T2-T0) / V2×0.0015%×0.01×1000kg / ton steel + (LF1 [Als]%-(T2-T0) / V2×0.0015%-LF2 [Als]%)×0.01×1000kg / ton steel.
[0055] Finally, the temperature reached 1675℃ and sample 2 was taken. LF2
Als
[0056] S3: RH refining.
[0057] S4: Continuous casting.
[0058] In the above method, the embodiment of the present invention uses aluminum particle diffusion deoxidation instead of aluminum iron precipitation deoxidation to achieve the best deoxidation and desulfurization effect in the slag washing process. 2 O 3The calculation method of the content can optimize the slag fluidity. Combined with the precise control of the Als content in the molten steel and the viscosity of the slag, the desulfurization effect can be further improved. The problems of low lime content in the CH1T ultra-low carbon cold heading slag, low Al2O3 content in the early LF slag, poor slag fluidity, weak interface reaction of the slag, and difficulty in removing sulfur from the molten steel are solved, which can effectively ensure the quality of the finished steel.
[0059] The beneficial effects of the CH1T ultra-low carbon cold heading steel and the preparation method thereof provided by the embodiments of the present invention are described in detail below in combination with specific embodiments, comparative examples and experimental examples.
[0060] Example 1
[0061] This embodiment provides a CH1T ultra-low carbon cold heading steel, which is prepared by the following method:
[0062] S1: Converter smelting, and the converter endpoint C is controlled at 0.04% to 0.05%, the endpoint O is controlled at 400 to 600ppm, P is controlled at ≤0.010%, and the tapping temperature is controlled at 1640±20℃; at the same time, slag washing slag and aluminum particles are added during converter smelting and tapping to perform converter tapping alloying and slag washing treatment. In the process, strong stirring argon gas of 60Nm 3 / h, the exposed diameter of molten steel is 55cm, the slag washing materials include lime akg / ton steel and fluorite bkg / ton steel, a is 7.2, b is 0.8; the amount of aluminum particles is ckg / ton steel, c is 1.7kg / ton steel;
[0063] At the same time, sampling can be done at the argon station before entering the station, and Als can be controlled at 0.020% to 0.040%, and the argon station [Als]% and argon station [S]% can be obtained;
[0064] S2: LF refining, including:
[0065] S21: Temperature measurement upon entering the station;
[0066] S22: Slagging is performed at the 8th gear, the heating rate is V1℃ / min, the slagging time is t1, and the slagging end temperature is T1. During the low-gear slagging process, argon gas is introduced at 35Nm 3 / h, the exposed diameter of molten steel is 28cm;
[0067] S23: Add W fluorite addition = 0.2 × (d1-1.5) kg / ton steel, and add W lime addition = 0.6 × (d1-1.5) kg / ton steel to adjust the slag viscosity;
[0068] S24: high-speed power transmission to the first preset temperature and strong stirring desulfurization; and specifically including after adjusting the slag viscosity, Al in the slag 2 O 3The content is 25% to 30%, and the cross-sectional thickness value d of the slag block on the slag sticking rod is in the range of 1.50-1.55mm. At the same time, electricity is sent to slag until the temperature of the molten steel reaches the first preset temperature T0, T0 is 1600℃±10℃, the heating rate of the high-grade power transmission process is V2℃ / min, and the slag-forming time is t2=(T0-T1) / V2. When the temperature of the molten steel reaches T0, strong stirring is turned on, and the strong stirring time S=5+(argon station [S]%-0.010%)÷0.010%×5, and the argon gas intake is 60 3 / h, the exposed diameter of molten steel is 55cm.
[0069] At the same time, the first addition of aluminum particles is carried out, and the addition amount G1 aluminum particles added = △ [Als] × 0.01kg / ton steel, △ [Als] = (t1 + t2) × 0.0015%; Al in the slag 2 O 3 The content of G furnace = (c% - argon station [Als]% - △ [Als] - △ [Als] 1) × 80%.
[0070] S25: Sampling, and continuing to send electricity at high gear to the second preset temperature. Specifically, after the strong stirring is completed, it also includes sampling to obtain LF1 [Als]% and LF1 [Mn]%, and continuing to send electricity to the second gear to the second preset temperature T2, T2 is 1675℃±5℃, and introducing argon gas 35~40Nm 3 / h, the exposed diameter of molten steel is 28cm; at the same time, the second addition of aluminum particles is carried out, and the mass of added aluminum particles G2 aluminum particles added = (T2-T0) / V2×0.0015%×0.01×1000kg / ton of steel + (LF1
Als
Als
[0071] S3: RH refining.
[0072] S4: Continuous casting.
[0073] In order to facilitate viewing of the various parameter information of Example 1, the various parameter information of Example 1 is first shown in Table 1:
[0074] Table 1. Parameter information in Example 1
[0075]
[0076]
[0077] Example 2
[0078] This embodiment provides a CH1T ultra-low carbon cold heading steel, and the difference between its preparation method and the preparation method provided in Example 1 is shown in Table 2:
[0079] Table 2. Parameter information in Example 2
[0080]
[0081]
[0082] Example 3
[0083] This embodiment provides a CH1T ultra-low carbon cold heading steel, and the difference between its preparation method and the preparation method provided in Example 1 is shown in Table 3:
[0084] Table 3. Parameter information in Example 3
[0085]
[0086]
[0087] Example 4
[0088] This embodiment provides a CH1T ultra-low carbon cold heading steel, and the difference between the preparation method thereof and the preparation method provided in Example 1 is that the strong stirring time during desulfurization is not obtained by calculation, resulting in insufficient strong stirring time, as shown in Table 4:
[0089] Table 4. Parameter information in Example 4
[0090]
[0091]
[0092] Comparative Example 1
[0093] Comparative Example 1 provides a CH1T ultra-low carbon cold heading steel, and the difference between its preparation method and the preparation method provided in Example 1 is that the composition of the slag washing slag material used is different, and is specifically shown in Table 5:
[0094] Table 5. Parameter information in Comparative Example 1
[0095]
[0096]
[0097] Comparative Example 2
[0098] Comparative Example 2 provides a CH1T ultra-low carbon cold heading steel, the preparation method of which is different from the preparation method provided in Example 1 in that fluorite and lime are not added to make the slag fluidity poor, and the specific results are shown in Table 6:
[0099] Table 6. Parameter information in Comparative Example 2
[0100]
[0101]
[0102] Comparative Example 3
[0103] Comparative Example 3 provides a CH1T ultra-low carbon cold heading steel, the preparation method of which is different from the preparation method provided in Example 1 in that no aluminum particles are added to make the slag fluidity poor, and the specific results are shown in Table 7:
[0104] Table 7. Parameter information in Comparative Example 3
[0105]
[0106]
[0107] Experimental Example 1
[0108] The sulfur content of the CH1T ultra-low carbon cold heading steel prepared in Examples 1-4 and Comparative Examples 1-3 was tested, and the test results are shown in Table 8.
[0109] Table 8. Sulfur content
[0110] project Sulfur content Example 1 0.003% Example 2 0.005% Example 3 0.006% Example 4 (Strong stirring time is not accurately calculated) 0.007% Comparative Example 1 (different slag washing materials) 0.011% Comparative Example 2 (without adding fluorite and lime) 0.009% Comparative Example 3 0.008%
[0111] According to the comparative data of Examples 1-4 and Comparative Examples 1-3 in Table 8, the embodiments of the present invention can be seen by 2 O 3 By controlling the content of and the cross-sectional thickness d of the slag block of the sticky slag rod, the fluidity of the corresponding slag at the desulfurization temperature can be adjusted to the best, so that the desulfurization efficiency and quality are fully improved to ensure the quality of the finished steel. At the same time, according to the comparison between Examples 1-3 and Example 4 in Table 8, the strong stirring efficiency and quality can be improved by accurately calculating the strong stirring time during desulfurization. According to the comparison between Examples 1-4 and Comparative Example 1 in Table 8, the use of 6.7-7.2 kg of lime / ton of steel, 0.8-1.0 kg of fluorite / ton of steel and 1.6-1.8 kg of aluminum particles / ton of steel provided by the embodiments of the present invention can effectively improve the desulfurization quality.
[0112] In summary, the embodiment of the present invention uses aluminum particle diffusion deoxidation instead of aluminum iron precipitation deoxidation to achieve the best deoxidation and desulfurization effect in the slag washing process. 2 O 3The calculation method of the content can optimize the slag fluidity. Combined with the precise control of the Als content in the molten steel and the viscosity of the slag, the desulfurization effect can be further improved. The problems of low lime content in the CH1T ultra-low carbon cold heading slag, low Al2O3 content in the early LF slag, poor slag fluidity, weak interface reaction of the slag, and difficulty in removing sulfur from the molten steel are solved, which can effectively ensure the quality of the finished steel.
[0113] In summary, the embodiments of the present invention provide a CH1T ultra-low carbon cold heading steel with high desulfurization efficiency and good effect and a preparation method thereof, which can effectively ensure the quality of the CH1T ultra-low carbon cold heading steel.
[0114] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing CH1T ultra-low carbon cold heading steel, It is characterized in that It includes converter smelting, LF refining, RH refining and continuous casting in sequence; Among them, slag washing slag and aluminum particles are added during converter smelting and steel tapping for converter steel tapping alloying and slag washing treatment, and in the LF refining process, when the molten steel temperature reaches the first preset temperature T0, strong stirring is turned on for desulfurization, T0 is 1600℃±10℃, and when strong stirring is turned on, the Al in the slag is controlled. 2 O 3 The content of is 25% to 30%, and the cross-sectional thickness value d of the slag block on the slag sticking rod is in the range of 1.50-1.55mm; After the steel is smelted in the converter, the method also includes sampling at the argon station to obtain the argon station [S]% in the molten steel; and the preparation method also includes determining the strong stirring time according to the argon station [S]% and the specified value 0.010% of the CH1T ultra-low carbon cold heading steel process card when the molten steel temperature reaches the first preset temperature; wherein, when the argon station [S]% is less than 0.010%, the strong stirring time is 5 minutes, and when the argon station [S]% is greater than 0.010%, the strong stirring time S=5+(argon station [S]%-0.010%)÷0.010%×5, in units of min; The slag washing material includes lime akg / ton steel and fluorite bkg / ton steel, a is 6.7-7.2, b is 0.8-1.0; the amount of aluminum particles is ckg / ton steel, c is 1.6-1.8; and LF refining includes temperature measurement at the station, low-speed electrification of slag, adjustment of slag viscosity, and high-speed electrification to the first preset temperature; Wherein, by adding the fluorite and the lime in the process of adjusting the viscosity of the slag, the cross-sectional thickness value d of the slag block on the slag sticking rod is controlled between 1.50-1.55 mm; and the added amount of the fluorite Wfluorite added = 0.2×(d1-1.5) kg / ton of steel, the added amount of the lime Wlime added = 0.6×(d1-1.5) kg / ton of steel, d1 is the real-time measurement value of the cross-sectional thickness of the slag block on the slag sticking rod; The heating rate of the low-speed power transmission slag-forming process is V1℃ / min, the slag-forming time is t1, and the slag-forming end temperature is T1; the heating rate of the high-speed power transmission process is V2℃ / min, and the slag-forming time is t2=(T0-T1) / V2; the argon gas flow rate of the high-speed power transmission and low-speed power transmission slag-forming is 35~40Nm³ / h, and the exposed diameter of the molten steel is 25cm~30cm; In addition, aluminum particles are added during the high-speed power transmission process to compensate for the aluminum content lost during the low-speed power transmission slag and high-speed power transmission process, so as to control the Al content in the slag. 2 O 3 The content is 25% to 30%; among them, the mass of the added aluminum particles G1 is determined by the aluminum content △【Als】 lost by power transmission and heating and the aluminum content lost during the strong stirring process △【Als】1, G1 aluminum particles added = △【Als】×0.01×1000kg / ton steel + △【Als】1×0.01×1000kg / ton steel, △【Als】=(t1+t2)×0.0015%,△【Als】1=S×0.003%; After the strong stirring is completed, it also includes sampling to obtain the aluminum content LF1 [Als]% and the manganese content LF1 [Mn]% in the molten steel after the strong stirring is completed; After the high-speed power transmission reaches the first preset temperature, the method further includes continuing to transmit power at the high-speed power transmission to the second preset temperature T2, where T2 is 1675°C±5°C; and in the process of continuing to transmit power at the high-speed power transmission, aluminum particles and low-carbon ferromanganese are added to adjust the aluminum content LF2 [Als]% in the molten steel to 0.005% to 0.009%, so as to control the manganese content LF2 [Mn]% in the molten steel to the process card target of 0.10%; In the process of continuing high-speed power transmission, the amount of argon gas introduced is 35~40Nm³ / h, the exposed diameter of molten steel is 25cm~30cm, and the heating rate is V2℃ / min; and the mass of aluminum particles to be added is determined based on the Als content lost during the heating process, LF1 [Als]%, and LF2 [Als]% G2 aluminum particle addition = (T2-T0) / V2×0.0015%×0.01×1000kg / ton steel + (LF1 [Als]%-(T2-T0) / V2×0.0015%-LF2 [Als]%)×0.01×1000kg / ton steel; The Als content of the aluminum particles added together with the slag washing slag material is c%; after the converter smelting steel, it also includes sampling at the argon station to obtain the argon station [Als]% in the molten steel, and the argon station [Als]% is controlled between 0.020% and 0.040%; The Al in the slag 2 O 3 The content G furnace is calculated by argon station [Als]%, c% and the loss of aluminum in molten steel e%, and G furnace = (c% - argon station [Als]% - e%) × 80%; wherein, e% is 0 before electro-slag is sent, and when electro-slag is sent to make the molten steel temperature reach the first preset temperature, e% = △ [Als] + △ [Als] 1.
2. The method for preparing CH1T ultra-low carbon cold heading steel according to claim 1, Features: When strong stirring is turned on, the argon gas flow rate is 55-65Nm³ / h and the exposed diameter of molten steel is 50cm-60cm.
3. The method for preparing CH1T ultra-low carbon cold heading steel according to claim 2, Features: When strong stirring is turned on, the argon gas flow rate is 60³ Nm³ / h and the exposed diameter of molten steel is 55cm.
4. The method for preparing CH1T ultra-low carbon cold heading steel according to claim 1, Features: LF final slag includes CaO: 52%~54%, SiO 2 :3%~5%,Al 2 O 3 : 25% to 30%, FeO: 0.7% to 0.8%, MnO: 0.2% to 0.3%, S: 0.3% to 0.5%, MgO: 5% to 7%, P 2 0 5 : 0.05~0.08%, R: 10~18, and W(FeO+MnO) in the LF final slag is <1%.
5. A CH1T ultra-low carbon cold heading steel, It is characterized in that The steel is prepared by the preparation method of CH1T ultra-low carbon cold heading steel described in any one of claims 1 to 4.
Citation Information
Patent Citations
Producing method of clean steel
CN101956040A
Production method of ultra-low-carbon, low-silicon, low-manganese and low-aluminum steel continuous casting blank
CN109943680A
Cold forging steel and production method thereof
CN113667882A
LF refining method of CH1T ultra-low carbon cold forging steel
CN115261560A
Production process for increasing continuous casting heats of aluminum-deoxidized high-carbon chromium bearing steel
WO2022267707A1