Graphene-loaded metal single atom composite material, preparation method and application

The preparation of graphene-supported metal single-atom composite materials solves the problem of easy oxidation and agglomeration of metal single-atom catalysts, achieves efficient degradation of phenolic pollutants, improves catalytic performance and stability, and is suitable for green and environmentally friendly sewage treatment.

CN116060002BActive Publication Date: 2024-10-18RES CENT FOR ECO ENVIRONMENTAL SCI THE CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310160629.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-10-18
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

In the existing technology, metal single-atom catalysts are prone to oxidation and agglomeration, resulting in reduced catalytic performance, making it difficult to synthesize stable single-atom catalysts on suitable carriers, affecting the activity and stability of persulfate, and thus affecting the degradation effect of phenolic pollutants. .

Method used

Through graphene-loaded metal single atom composite materials, the graphene material is used to anchor the metal single atom active center, and combined with hydrothermal carbonization and high-temperature carbon thermal shock technology, a composite material in which metal single atoms are evenly dispersed is prepared to achieve the stability of metal single atoms. anchoring and high catalytic performance.

Benefits of technology

It improves the activity and stability of catalytic persulfate, effectively degrades phenolic pollutants in organic wastewater, and achieves green and environmentally friendly sewage purification. It has good catalytic performance, low cost, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116060002B_ABST
    Figure CN116060002B_ABST
Patent Text Reader

Abstract

The present disclosure proposes a graphene-loaded metal single-atom composite material, comprising: graphene material, metal single atoms, uniformly dispersed in the graphene material, and having catalytic degradation performance, wherein the metal single-atom material contains a metal active center that coordinates with the graphene material to achieve the anchoring of the metal single-atom material on the graphene material. The present disclosure also proposes a method for preparing the aforementioned composite material, comprising: adding a biomass material to a metal-soluble salt solution for mixing; then a hydrothermal carbonization reaction occurs, so that the active metal coordinates with the oxygen-containing functional group to form a hydrothermal carbon with uniform metal loading; then a high-temperature carbon thermal shock reaction occurs, so that the metal active center interacts with the carbon substrate to form a stable coordination structure, so as to achieve the anchoring of the metal single atom on the graphene material, and after cooling, a graphene-loaded metal single-atom composite material is obtained. The present disclosure also proposes a method for degrading organic matter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of graphene material preparation, and in particular to a graphene-loaded metal single-atom composite material, a preparation method and an application thereof. Background Art

[0002] Phenol compounds are basic raw materials in the organic chemical industry and are widely used in industry. Effective degradation of them has application value and far-reaching social effects in environmental governance.

[0003] Advanced Oxidation Process (AOPs) can directly mineralize organic pollutants or improve the biodegradability of pollutants through oxidation. It also has great advantages in the treatment of trace harmful chemicals such as environmental hormones. It can completely mineralize or decompose most organic matter and has good application prospects. Among them, persulfate advanced oxidation technology has attracted widespread attention due to its strong oxidation ability and the advantages of not producing sludge. However, in persulfate advanced oxidation technology, a catalyst is required to activate the oxidation and decomposition performance of persulfate.

[0004] Single-atom catalysts, with their unique structure, have the highest atomic utilization efficiency and metal centers with high catalytic performance, and can be used as ideal catalysts for activating persulfate to oxidize organic pollutants. However, the synthesis of metal single atoms is challenging due to their own instability, easy deactivation, and the need for doping with exogenous heteroatoms to assist coordination. Single-atom catalysts synthesized in related technologies are susceptible to surface oxidation and metal agglomeration, which reduces the catalytic efficiency. Therefore, the synthesis of stable single-atom catalysts on suitable carriers is a problem that needs to be solved urgently. Summary of the invention

[0005] In view of this, in order to solve the problem that metal single-atom catalysts are easily oxidized and agglomerated, thereby reducing the catalytic performance, the present disclosure proposes a graphene-loaded metal single-atom composite material, a preparation method and an application, in order to improve the activity and stability of the catalytic persulfate by anchoring the metal single-atom active center on the graphene carrier, thereby degrading phenol pollutants in organic wastewater and achieving wastewater purification in a green and environmentally friendly manner.

[0006] In one aspect of the present disclosure, the present disclosure provides a graphene-supported metal single-atom composite material, comprising:

[0007] Graphene materials;

[0008] Metal single atoms are evenly dispersed in graphene materials and have catalytic degradation properties;

[0009] Among them, the metal single atom material contains a metal active center and is coordinated with the graphene material to achieve the anchoring of the metal single atom material on the graphene material.

[0010] According to the embodiment of the present disclosure, the number of layers of the graphene material is 1 to 5, and it is prepared based on waste biomass materials.

[0011] According to the embodiment of the present disclosure, the metal loading amount of the graphene-loaded metal single-atom composite material is 3-10%.

[0012] In another aspect of the present disclosure, the present disclosure provides a method for preparing the aforementioned composite material, comprising:

[0013] adding biomass material to a metal soluble salt solution and mixing to obtain a reaction mixture;

[0014] Under the first reaction temperature condition, the reaction mixture undergoes a hydrothermal carbonization reaction, so that the active metal is coordinated with the oxygen-containing functional group to form a hydrothermal carbon precursor with uniform metal loading;

[0015] Under the conditions of the second reaction temperature and inert gas atmosphere, the hydrothermal carbon precursor is converted into graphene material under the high-temperature carbon thermal shock reaction, providing activation energy for the dispersion of metal single atoms, allowing the metal active centers to interact with the carbon substrate to form a stable coordination structure, so as to achieve the anchoring of metal single atoms on the graphene material, and after cooling, a graphene-loaded metal single atom composite material is obtained.

[0016] According to an embodiment of the present disclosure, the metal soluble salt includes at least one of the following: an iron salt, a cobalt salt, a nickel salt, and a copper salt;

[0017] The particle size of the biomass material is less than 200 mesh.

[0018] According to an embodiment of the present disclosure, the mass ratio of metal to biomass material is 1:7 to 1:20.

[0019] According to an embodiment of the present disclosure, the first reaction temperature condition includes 210-220°C;

[0020] The duration of the hydrothermal carbonization reaction ranges from 10 to 12 h;

[0021] The mass ratio of the biomass material to the metal soluble salt solution is 1:10.

[0022] According to an embodiment of the present disclosure, the second reaction temperature condition includes heating to 3000° C. within 480 ms to 520 ms;

[0023] The heating rate of high temperature carbon thermal shock reaction is 3.75~6℃ / ms.

[0024] According to an embodiment of the present disclosure, the biomass material includes corn stover.

[0025] In another aspect of the present disclosure, the present disclosure provides a method for catalytically degrading phenolic pollutants, comprising:

[0026] The graphene-loaded metal single-atom composite material is dispersed in an aqueous solution containing phenolic pollutants, and persulfate is added and mixed to decompose the phenolic pollutants.

[0027] According to the embodiments of the present disclosure, the present disclosure constructs a composite material with graphene as a carrier and metal single atoms uniformly and stably loaded, wherein the graphene is made from waste biomass materials. In the composite process, the number of graphene layers prepared is 1 to 5 layers without doping with exogenous heteroatoms through hydrothermal carbonization technology and high-temperature carbon thermal shock technology, which can make the metal single atoms fully dispersed and have high catalytic performance. At the same time, the metal loading of the metal single atom catalyst in the composite material proposed in the present disclosure is between 3 and 10%, which reduces the tendency of metal atom clusters, takes metal single atoms as the main active center, has a good effect of activating persulfate to degrade organic pollutants, is green, environmentally friendly, non-toxic and harmless.

[0028] According to the embodiments of the present disclosure, the present disclosure uses environmentally friendly and cheap waste biomass as a carbon source, and forms porous hydrothermal carbon with rich surface functional groups through hydrothermal carbonization treatment. In the hydrothermal process, the active metal ions are coordinated with the rich oxygen-containing functional groups on the surface of the hydrothermal carbon by means of high temperature and high pressure coupling, forming a hydrothermal carbon precursor with uniform metal load; then the hydrothermal carbon is converted into graphene material through a high-temperature carbon thermal shock process, which provides activation energy for the dispersion of metal single atoms, so that the metal active center interacts with the carbon substrate to form a stable coordination structure, and the anchoring of metal single atoms on the graphene substrate is achieved without doping with other heteroatoms. In this preparation method, the metal loading is high, the catalytic performance is good, the technical route is simple, the process is fast and efficient, and the cost is low. It has the advantages of environmental protection and controllability, which is conducive to mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the process of preparing the graphene-supported metal single-atom composite material disclosed in the present invention;

[0030] Figure 2 is the XRD diagram of the graphene-supported metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure;

[0031] Figure 3 is an infrared spectrum of the graphene-supported metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure;

[0032] Figure 4 is a Raman spectrum of the graphene-supported metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure;

[0033] Figure 5 is a scanning electron microscope image of the graphene-supported metallic iron single-atom composite material prepared in Example 2 of the present disclosure;

[0034] Figure 6 This is a spherical aberration electron microscope image of the graphene-supported metallic iron single-atom composite material prepared in Example 2 of the present disclosure;

[0035] Figure 7 This is a spherical aberration electron microscope image of a graphene-loaded composite material of a small amount of metallic iron single atoms prepared in Comparative Example 1 of the present disclosure;

[0036] Figure 8 This is a spherical aberration electron microscope image of the graphene-supported metallic iron cluster composite material prepared in Comparative Example 2 of the present disclosure;

[0037] Fig. 9 This is a spherical aberration electron microscope image of the graphene-loaded metal iron composite material prepared in Comparative Example 3 of the present disclosure;

[0038] Fig.10 This is a spherical aberration electron microscope image of the graphene-loaded metal iron composite material prepared in Comparative Example 4 of the present disclosure;

[0039] Fig.11 It is a degradation curve diagram of bisphenol A degradation by persulfate activation of the graphene-supported metal single-atom composite material prepared in Examples 1, 2, 3 and Comparative Examples 1 and 2 of the present disclosure. DETAILED DESCRIPTION

[0040] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0041] The endpoints and any values ​​of the ranges disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this disclosure.

[0042] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0043] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification, and should not be interpreted in an idealized or overly rigid manner.

[0044] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present disclosure shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. If the full text involves descriptions such as "first", "second", etc., the descriptions such as "first", "second", etc. are only used to distinguish similar objects, and cannot be understood as indicating or implying their relative importance, order of precedence, or implicitly indicating the number of technical features indicated. It should be understood that the data described by "first", "second", etc. can be interchangeable under appropriate circumstances.

[0045] In the present disclosure, the term "single atom catalyst" refers to a material in which a metal is supported in the form of a single atom on a carrier such as a metal, a metal oxide, a two-dimensional material, and a molecular sieve, and a single atom is used as a catalytic active center for catalytic action. The advantages of the single atom are that it has the characteristics of sharply increased surface free energy, quantum size effect, unique electronic structure, and unsaturated coordination environment, which effectively increase the active catalytic sites and atomic utilization rate. However, the single atom level causes a sharp increase in the surface free energy of the metal, and it is easy to agglomerate and couple to form metal clusters during preparation and reaction, resulting in catalyst deactivation.

[0046] In this disclosure, the term "graphene material" refers to carbon atoms in the form of sp 2 Carbon nanomaterials with a single-layer two-dimensional honeycomb lattice structure formed by hybrid stacking have a high specific surface area and a unique planar structure, and are widely used in energy, materials, environment and other fields. The preparation methods of graphene materials include mechanical exfoliation, chemical vapor deposition, redox method, etc., but there are problems such as cumbersome steps in mass production, expensive precursors and a large amount of solvents, and the high chemical stability of the generated graphene materials, which are not easy to recombine with active centers.

[0047] In the related art, it is difficult for carbon-based materials to coordinate with metals, and other materials such as nitrogen and oxygen need to be introduced to reduce the activation energy. At the same time, the clustering tendency of single-atom metals makes the metal loading low and the dispersion uneven. In order to ensure the catalytic performance, the metal loading of conventional carbon-based material-supported metal catalysts is usually less than 1%.

[0048] In the process of realizing the present disclosure, it was found that the graphene-loaded metal single-atom composite material prepared by the present disclosure is not doped with other heteroatoms, the metal loading amount is increased, and the distribution of the metal single-atom material is uniform and stable, compared with the existing graphene-loaded metal material, so that the catalytic performance of the composite material is good and stable.

[0049] In one aspect of the present disclosure, the present disclosure provides a graphene-supported metal single-atom composite material, comprising:

[0050] Graphene materials;

[0051] Metal single atoms are evenly dispersed in graphene materials and have catalytic degradation properties;

[0052] Among them, the metal single atom material contains a metal active center and is coordinated with the graphene material to achieve the anchoring of the metal single atom material on the graphene material.

[0053] According to the embodiments of the present disclosure, the present disclosure constructs a composite material with graphene as a carrier and metal single atoms uniformly and stably loaded, wherein the graphene is made from waste biomass materials. The graphene material provides activation energy for the dispersion of metal single atoms, so that the metal single atoms are uniformly dispersed, and the metal active centers interact with the carbon substrate to form a stable coordination structure, and the anchoring of metal single atoms on the graphene substrate is achieved without doping other heteroatoms. It reduces the tendency of metal atom clusters, has a good effect of activating persulfate to degrade organic pollutants, is green and environmentally friendly, and is non-toxic and harmless.

[0054] According to the embodiment of the present disclosure, the number of layers of the graphene material is 1 to 5, and it is prepared based on waste biomass materials.

[0055] According to the embodiments of the present disclosure, the number of graphene layers prepared is 1 to 5, which can fully disperse metal atoms and have high catalytic performance; the use of waste biomass materials is environmentally friendly, green, safe and harmless.

[0056] According to the embodiment of the present disclosure, the metal loading amount of the graphene-loaded metal single-atom composite material is 3-10%.

[0057] According to the embodiments of the present disclosure, the metal loading in the composite material proposed in the present disclosure is between 3% and 10%. Within this metal doping range, the metal single atoms are evenly and stably dispersed, reducing the tendency of metal atom clusters, and having a good effect of activating persulfate to degrade organic pollutants. It is green, environmentally friendly, non-toxic and harmless.

[0058] Figure 1 It is a schematic diagram of the process of preparing the graphene-loaded metal single-atom composite material disclosed in the present invention.

[0059] In another aspect of the present disclosure, the present disclosure provides a method for preparing the aforementioned composite material, such as Figure 1 As shown, including:

[0060] adding biomass material to a metal soluble salt solution and mixing to obtain a reaction mixture;

[0061] Under the first reaction temperature condition, the reaction mixture undergoes a hydrothermal carbonization reaction, so that the active metal is coordinated with the oxygen-containing functional group to form a hydrothermal carbon precursor with uniform metal loading;

[0062] Under the conditions of the second reaction temperature and inert gas atmosphere, the hydrothermal carbon precursor is converted into graphene material under the high-temperature carbon thermal shock reaction, providing activation energy for the dispersion of metal single atoms, so that the metal active center interacts with the carbon substrate to form a stable coordination structure, so as to realize the anchoring of metal single atoms on the graphene material, and after cooling, a graphene-loaded metal single atom composite material is obtained.

[0063] According to the embodiments of the present disclosure, the present disclosure uses environmentally friendly and cheap waste biomass as a carbon source, forms porous hydrothermal carbon with rich surface functional groups through hydrothermal carbonization treatment, and coordinates metals with oxygen-containing functional groups through high temperature and high pressure reactions in aqueous solution to form a hydrothermal carbon precursor with uniform metal load. During the initial heating stage of high-temperature carbon thermal shock, the mobility of the centroid particles in the hydrothermal carbon precursor is reduced, and the surrounding amorphous carbon undergoes rapid graphitization to form a graphene-like coating covering the centroid particles, converting the hydrothermal carbon into a graphene material. During the metal dispersion and single-atom synthesis process, the high-temperature carbon thermal shock provides activation energy for single-atom dispersion by forming thermodynamically stable metal-defect bonds, and the cooling process ensures the overall stability of the material, which plays an important role in the uniform dispersion of single atoms.

[0064] According to the disclosed embodiments, during the formation of graphene-loaded single-atom composite materials, metal active centers interact with carbon substrates, metal salts decompose at high temperatures, other substances are released in gaseous form, and metal droplets move rapidly and split on the substrate surface, uniformly dispersing while promoting rapid graphitization of the carbon substrate. The surface defect structure of graphene provides a good coordination environment for the metal, forming a stable coordination structure with metal single atoms, and realizing the anchoring of single atoms on the graphene substrate without doping with other heteroatoms. The preparation method has a simple technical route, a fast and low-cost process, and has the advantages of environmental protection and controllability, which is conducive to mass production.

[0065] According to an embodiment of the present disclosure, the metal soluble salt includes at least one of the following: iron salt, cobalt salt, nickel salt, copper salt; and the particle size of the biomass material is less than 200 mesh.

[0066] According to the embodiments of the present disclosure, it was found in the study that too low a metal content would cause the graphene-loaded metal single-atom composite material to have weaker reaction activity, and too high a metal content would cause the metal to agglomerate to form clusters, thereby reducing the catalytic activity.

[0067] According to the embodiment of the present disclosure, the mass ratio of metal to biomass material includes 1:7 to 1:20, for example, it can be 1:7, 1:10, 1:16, 1:20, etc. According to the embodiment of the present disclosure, the mass ratio of metal to biomass material is within the range of 1:7 to 1:20, and the metal loading of the composite material is between 3% and 10%. Figure 6 As shown, a graphene-supported metal single-atom composite material is obtained; Figure 7 As shown, when the metal content is too low, there is almost no metal single atom material, and the catalytic activity is weak, such as Figure 8 As shown, too high a metal content will cause metals to aggregate into clusters, reducing the catalytic activity.

[0068] According to an embodiment of the present disclosure, the first reaction temperature condition includes 210-220°C, for example, it can be selected as 210°C, 215°C, 220°C, etc.; the duration of the hydrothermal carbonization reaction includes 10-12h, for example, it can be selected as 10h, 11h, 12h, etc.; the mass ratio of the biomass material to the metal soluble salt solution includes 1:10.

[0069] According to an embodiment of the present disclosure, the second reaction temperature condition includes heating to 3000°C within 480ms~520ms; the heating rate of the high-temperature carbon thermal shock reaction is 3.75~6°C / ms, for example, it can be selected as 3.75°C / ms, 4°C / ms, 5.5°C / ms, 6°C / ms, etc.

[0070] According to the embodiments of the present disclosure, the temperature and time of the reaction can be adjusted by changing the current and voltage parameters to control the morphology of the metal single atom material and form a graphene material. Figure 6 As shown, within the above conditions, a graphene-supported metal single-atom composite material is obtained; Fig. 9 , Fig.10 As shown, if the heating rate and shock temperature do not meet the requirements, metal atoms will aggregate to form clusters, reducing the catalytic performance.

[0071] According to an embodiment of the present disclosure, the biomass material includes corn stover.

[0072] In another aspect of the present disclosure, the present disclosure provides a method for catalytically degrading phenolic pollutants, comprising:

[0073] The graphene-loaded metal single-atom composite material is dispersed in an aqueous solution containing phenolic pollutants, and persulfate is added and mixed to decompose the phenolic pollutants.

[0074] According to the embodiments of the present disclosure, phenols are the main pollutants in industrial wastewater. The method proposed in the present disclosure is used to directly degrade phenol pollutants in industrial wastewater by catalyzing the decomposition of persulfate to produce free radicals. The degradation process does not require additional enrichment and separation operations, and is fast, efficient, and green and environmentally friendly.

[0075] It should be noted that the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments of the present disclosure, other embodiments obtained by ordinary technicians in the field without creative work are all within the scope of protection of the present disclosure.

[0076] The corn stalks used in the present invention were taken from a certain city, FeCl3·6H2O (analytical grade) was purchased from Sinopharm Chemical Reagent Co., Ltd., ultrapure water (resistivity of 18.2 MΩ·cm) was prepared by the laboratory HHitech ultrapure water instrument, potassium persulfate (≥42% KHSO5) was purchased from Aladdin Biochemical Technology Co., Ltd., and bisphenol A (chromatographic grade) was purchased from Shanghai McLean Biochemical Technology Co., Ltd.

[0077] Example 1

[0078] S1: Dissolve 1 g of metal soluble salt FeCl3·6H2O in 40 mL of ultrapure water, add 4 g of corn stalks with a mesh size less than 200 to the solution, and the theoretical metal loading is 5%. Ultrasonic treatment is performed for 20 min, and after thorough mixing, a mixture of metal salt solution and corn stalks is obtained;

[0079] S2: Transfer the mixture in S1 to a 100 mL polytetrafluoroethylene-lined autoclave, set the hydrothermal carbonization reaction temperature to 210°C, the reaction time to 10 h, and the solid-liquid ratio to 1:10. After the hydrothermal treatment is completed and cooled to room temperature, the solid hydrothermal product is separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0080] S1: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was then installed in a heating chamber. After evacuation, the heating voltage was set to 40 V and the current was 500 A in an inert gas argon atmosphere. The temperature was raised to 3000 °C in 500 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a composite material of graphene-loaded metallic iron single atoms.

[0081] Embodiment 2:

[0082] S1: 2 g of metal soluble salt FeCl3·6H2O was dissolved in 40 mL of ultrapure water, and 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 10%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of metal salt solution and corn stalks.

[0083] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0084] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current was 500 A. The temperature was increased to 3000 °C in 500 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, it was cooled to room temperature to obtain a composite material of graphene loaded with metallic iron single atoms.

[0085] Example 3

[0086] S1: 3 g of metal soluble salt FeCl3·6H2O was dissolved in 40 mL of ultrapure water, and then 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 15%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of the metal salt solution and the corn stalks.

[0087] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0088] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current was 500 A. The temperature was increased to 3000 °C in 500 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a composite material of graphene-loaded metallic iron nanoparticles.

[0089] Example 4

[0090] S1: 0.8 g of metal soluble salt NiCl2·6H2O was dissolved in 40 mL of ultrapure water, and 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 5%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of metal salt solution and corn stalks.

[0091] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0092] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was then installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current to 500 A. The temperature was increased to 3000 °C in 500 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a composite material of graphene loaded with single metal nickel atoms.

[0093] The following comparative example is that the theoretical metal loading of the composite material is not between 3 and 15%. After physical and chemical characterization and performance testing, it is verified that the graphene-loaded metal single-atom composite material with a metal loading between 3 and 10% has the best catalytic performance.

[0094] Comparative Example 1

[0095] S1: 0.2 g of metal soluble salt FeCl3·6H2O was dissolved in 40 mL of ultrapure water, and 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 1%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of metal salt solution and corn stalks.

[0096] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0097] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was then installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current to 500 A. The temperature was increased to 3000 °C in 500 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a composite material of graphene loaded with a small amount of metallic iron single atoms.

[0098] Comparative Example 2

[0099] S1: 5 g of metal soluble salt FeCl3·6H2O was dissolved in 40 mL of ultrapure water, and then 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 25%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of metal salt solution and corn stalks;

[0100] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0101] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current was 500 A. The temperature was increased to 3000 °C in 500 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a composite material of graphene-loaded metallic iron clusters.

[0102] Comparative Example 3

[0103] S1: 2 g of metal soluble salt FeCl3·6H2O was dissolved in 40 mL of ultrapure water, and 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 10%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of metal salt solution and corn stalks.

[0104] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0105] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current was 500 A. The temperature was increased to 1500 °C in 250 ms at a heating rate of 6000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a graphene-loaded metallic iron composite material.

[0106] Comparative Example 4

[0107] S1: 2 g of metal soluble salt FeCl3·6H2O was dissolved in 40 mL of ultrapure water, and 4 g of corn stalks with a mesh size less than 200 were added to the solution, with a theoretical metal loading mass fraction of 10%. The mixture was ultrasonically treated for 20 min and fully mixed to obtain a mixture of metal salt solution and corn stalks.

[0108] S2: The mixture in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the hydrothermal carbonization reaction temperature was set to 210°C, the reaction time was 10 h, and the solid-liquid ratio was 1:10. After the hydrothermal treatment was completed and cooled to room temperature, the solid hydrothermal product was separated by vacuum filtration, washed with ultrapure water and anhydrous ethanol, and dried overnight in a constant temperature blast drying oven at 60°C to obtain a hydrothermal carbon precursor with uniform metal loading;

[0109] S3: 50 mg of the hydrothermal carbon precursor in S2 was loaded into a graphite tube and squeezed and sealed with a graphite electrode, which was then installed in a heating chamber. After evacuation, in an inert gas argon atmosphere, the heating voltage was set to 40 V and the current was 500 A. The temperature was increased to 3000 °C in 3 seconds at a heating rate of 1000 °C / s for high-temperature carbon thermal shock. After the reaction was completed, the tube was cooled to room temperature to obtain a graphene-loaded metallic iron composite material.

[0110] Test Example 1 Morphology and Physical and Chemical Properties

[0111] The microscopic morphology and physicochemical properties of graphene materials were analyzed by X-ray diffraction, Fourier transform infrared spectroscopy, Raman spectroscopy, scanning electron microscopy, and spherical aberration electron microscopy.

[0112] Figure 2 3 is the XRD diagram of the graphene-supported metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure.

[0113] like Figure 2 As shown, the XRD curve shows the characteristic peak of carbon element in the graphene material, and there is no obvious characteristic peak of metallic iron element, which proves that the metal element in the graphene-loaded metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure exists as a single atom.

[0114] Figure 3 is an infrared spectrum of the graphene-supported metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure;

[0115] like Figure 3 As shown, the infrared curve shows the existence of chemical bonds such as C=C and C=C=O in the graphene-loaded metal single-atom composite materials prepared in Examples 1, 2, and 3 of the present disclosure, which can serve as coordination binding sites.

[0116] Figure 4It is a Raman spectrum diagram of the graphene-loaded metal single-atom composite material prepared in Examples 1, 2, and 3 of the present disclosure.

[0117] like Figure 4 As shown in the figure, the value of the parameter 2D / G is 1.1, proving that the carbon material prepared in the present disclosure is a graphene material. In addition, the curve shows that the graphene material has a strong defect peak, which can be used to coordinate and fix with the metal material through the metal-defect bond.

[0118] Figure 5 This is a scanning electron microscope image of the graphene-loaded metal single-atom composite material prepared in Example 2 of the present disclosure.

[0119] like Figure 5 As shown in the figure, a gray small particle structure is attached to the lamellar structure, which verifies that the composite material prepared in Example 2 of the present disclosure is composed of metal single-atom material (i.e., the gray small particle structure in the figure) and graphene material (i.e., the lamellar structure in the figure).

[0120] Figure 6 This is a spherical aberration electron microscope image of the graphene-loaded metal single-atom composite material prepared in Example 2 of the present disclosure.

[0121] like Figure 6 As shown, the bright spot structure in the figure is a metal single atom material, which further verifies the existence of metal iron single atoms and graphene layered structure in the composite material.

[0122] Figure 7 This is a spherical aberration electron microscope image of the graphene-loaded small amount of metallic iron single-atom composite material prepared in Comparative Example 1 of the present disclosure.

[0123] like Figure 7 As shown, the bright spot structure in the figure is a metal single atom material, indicating that under the condition of a metal loading of 1%, there is almost no metal iron single atom material.

[0124] Figure 8 This is a spherical aberration electron microscope image of the graphene-loaded metallic iron cluster composite material prepared in Comparative Example 2 of the present disclosure.

[0125] like Figure 8 As shown, the bright spot structure in the figure is a metallic iron cluster organization, indicating that under the condition of a metal loading of 25%, the metallic iron atoms agglomerate to form a cluster structure due to the excessive loading.

[0126] Fig. 9 This is a spherical aberration electron microscope image of the graphene-loaded metal iron composite material prepared in Comparative Example 3 of the present disclosure.

[0127] like Fig. 9As shown, the bright spot structure in the figure is a metallic iron cluster organization, indicating that during the high-temperature carbon thermal shock process, when the temperature is lower than 3000°C, the metallic iron atoms will agglomerate to form a cluster structure.

[0128] Fig.10 This is a spherical aberration electron microscope image of the graphene-loaded metal iron composite material prepared in Comparative Example 4 of the present disclosure.

[0129] like Fig.10 As shown, the bright spot structure in the figure is a metallic iron cluster organization, indicating that when the heating rate is too slow during the high-temperature carbon thermal shock process, the metallic iron atoms will agglomerate to form a cluster structure.

[0130] Test Example 2 Catalytic Performance

[0131] 10 mg of catalyst was dispersed in 50 mL of 20 mg / L bisphenol A (BPA) solution, and the pH of the test solution was 6.5. Before the reaction started, the solution was stirred for 30 min to reach adsorption equilibrium, and then 20 mg of persulfate (PMS) was added to the dispersion to start the reaction. Every 5 min, 4 mL of sample was passed through a 0.22 μm filter membrane and placed in a 5 mL centrifuge tube, and 0.5 mL of methanol was added to capture the residual free radicals in the solution. The concentration of bisphenol A solution was measured at a wavelength of 276 nm using a Shimadzu UV-1800 ultraviolet-visible spectrophotometer from Japan, and the concentration ratio before and after the bisphenol A test was used as a parameter to characterize the degradation rate.

[0132] Fig.11 It is a degradation curve diagram of bisphenol A degradation by persulfate activation of the graphene composite material prepared in Examples 1, 2, 3 and Comparative Examples 1 and 2 of the present disclosure.

[0133] like Fig.11 As shown, the graphene-supported metal single-atom composite material prepared in the present invention has good performance in catalyzing persulfate, and the degradation efficiency of phenol pollutants can reach more than 80% within 30 minutes, among which the graphene-supported metal single-atom composite material with a theoretical metal loading of 10% has the best catalytic performance.

[0134] Furthermore, the test results show that the catalytic effect of graphene composite materials with metal loading not in the range of 3-10% is poor. The reason is that too low metal loading will reduce the content of metal single atoms, reducing the catalytic performance of the composite material; too high metal loading will load a large amount of metal substances, and metal atoms will attract and couple with each other with large surface free energy to form metal clusters, reducing the catalytic activity of the composite material.

[0135] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a graphene-loaded metal single-atom composite material, comprising: Adding biomass material to a metal soluble salt solution and mixing to obtain a reaction mixture, wherein the metal soluble salt includes at least one of the following: iron salt, cobalt salt, nickel salt, copper salt; Under the first reaction temperature condition, the reaction mixture undergoes a hydrothermal carbonization reaction, so that the active metal is coordinated with the oxygen-containing functional group to form a hydrothermal carbon precursor with uniform metal loading, wherein the first reaction temperature condition is 210-220° C.; Under the conditions of a second reaction temperature and an inert gas atmosphere, the hydrothermal carbon precursor is converted into a graphene material under a high-temperature carbon thermal shock reaction, providing activation energy for the dispersion of metal single atoms, so that the metal active center interacts with the carbon substrate to form a stable coordination structure, so as to achieve the anchoring of the metal single atom on the graphene material, and after cooling, the graphene-loaded metal single atom composite material is obtained, wherein the second reaction temperature condition is to heat up to 3000° C. within 480 ms to 520 ms, and the heating rate of the high-temperature carbon thermal shock reaction is 3.75 to 6° C. / ms; The mass ratio of the metal to the biomass material is 1:7 to 1:20, and the metal loading amount of the graphene-loaded metal single-atom composite material is 3 to 10%.

2. The method according to claim 1, wherein: The particle size of the biomass material is less than 200 meshes.

3. The method according to claim 1, wherein: The duration of the hydrothermal carbonization reaction is 10 to 12 hours; The mass ratio of the biomass material to the metal soluble salt solution is 1:

10.

4. The method according to claim 1, wherein: The biomass material includes corn stover.

5. A graphene-supported metal single-atom composite material obtained by the preparation method according to any one of claims 1 to 4, comprising: Graphene materials; Metal single atoms are uniformly dispersed in the graphene material and have catalytic degradation properties; Wherein, the metal single atom material contains a metal active center that coordinates with the graphene material to achieve anchoring of the metal single atom material on the graphene material; The metal loading amount of the graphene-loaded metal single-atom composite material is 3-10%.

6. The composite material according to claim 5, wherein The graphene material is prepared based on waste biomass materials; The number of layers of the graphene material is 1 to 5.

7. A method for catalytic degradation of phenolic pollutants, comprising: The graphene-supported metal single-atom composite material according to any one of claims 5 or 6 is dispersed in an aqueous solution containing phenolic pollutants, and persulfate is added and mixed to decompose the phenolic pollutants.

Citation Information

Patent Citations

  • A preparation method of graphitized carbon nano material

    CN101445234A

  • Method for preparing fewer-layer graphene on basis of biomass waste

    CN105060289A

  • Method for preparing metal particle-loaded coal-based graphene through high-temperature thermal shock

    CN113333773A

  • Nitrogen-doped graphene nickel-iron bimetallic monatomic catalyst for directly activating persulfate to treat phenolic wastewater