Alkali-activated slag-tannery sludge solidifying agent and its mixing ratio optimization method
By optimizing the mixing ratio of alkali-activated slag-tannery sludge solidifying agent through response surface analysis, the problem of environmental pollution caused by incineration and landfilling and the leaching of hexavalent chromium from cement solidified bodies in acidic environments was solved, achieving high strength. The solidification and resource utilization of sludge reduces costs and carbon emissions.
Patent Information
- Application Number
- CN202310015105.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-01-05
AI Technical Summary
The existing methods of incineration and landfilling can easily cause environmental pollution and secondary pollution. It is difficult for the cement solidified body to inhibit the leaching of hexavalent chromium in an acidic environment, causing environmental harm.
An alkali-activated slag-tannery sludge solidifying agent material based on RSM is used, the mix ratio is optimized through response surface analysis, a regression model is established, and physical and chemical characterization is performed using testing methods such as XRD and SEM-EDS to achieve microscopic solidification of sludge.
A high-strength alkali-activated slag-tannery sludge solidifying agent has been realized to effectively solidify heavy metal ions and avoid secondary pollution. The cost is lower than traditional cement and meets the requirements of environmentally friendly materials.
Smart Images

Figure CN116063018B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the building material technology, and in particular relates to an alkali-activated slag-tannery sludge solidifying agent material based on RSM and a method for optimizing the mixing ratio thereof. Background Art
[0002] At present, according to statistics, about 60-80 tons of sewage and 150 kg of sludge (water mass fraction of 95%-98%) are produced for every ton of cowhide produced. The solid waste generated in the leather production process and the sludge generated in the leather wastewater treatment process are leather sludge. Leather sludge is usually considered as hazardous waste because of its high chromium (Cr) ion content. The main source of chromium in leather sludge is obtained by separating it from chrome tanning wastewater when chrome tanning wastewater is deposited with lime (CaO) and flocculants (Kavouras et al., 2015). At present, the main treatment methods for leather sludge are incineration and landfill. Although incineration is widely used (Alibardi and Cossu, 2016; Zupancic and Jemec, 2010), it has certain limitations. Trivalent chromium is converted into hexavalent chromium at high temperature, and hexavalent chromium is highly toxic and will cause heavy metal chromium poisoning in people as it accumulates in the food chain. Landfill is only appropriate when heavy metal emissions are below safety standards; if not handled properly, it will cause serious environmental pollution and secondary pollution. Therefore, heavy metals need to be solidified (Cossu, 2010) before they can be used for landfill.
[0003] As an effective method for treating hazardous waste (Shi and Fernandez-Jimenez, 2006), the solidification method has the advantages of short treatment time, low cost, good effect and wide application range. It is evaluated by the US Environmental Protection Agency as the most effective technology for treating hazardous waste. At present, the most commonly used solidifying agent in solidification / stabilization technology is cement. However, due to its poor acid resistance and high permeability, heavy metal chromium cannot be completely sealed in the solidified body. It is difficult to inhibit the leaching of hexavalent chromium in an acidic environment, which causes harm to the environment. In contrast, geopolymer is an inorganic gelling material with a three-dimensional network structure. It has a simple process, little environmental pollution, and low energy consumption. It also has the advantages of high strength, corrosion resistance, and low permeability. It has excellent performance in solidifying heavy metal ions. In addition, the raw materials of geopolymers are widely available, and a large amount of industrial waste residues (such as fly ash, slag, etc.) can be used to prepare geopolymers. As a new type of inorganic polymer, geopolymer has a cage-like zeolite structure. Their basic structure is SiO4 tetrahedron and AlO4 tetrahedron (Davidovits, 1991). They are the products of the reaction of solid aluminum silicate with high concentrations of alkali and silicate, and are amorphous or semi-crystalline materials (Guoetal, 2017). Geopolymers have high compressive strength and low permeability and are considered to be a solidification system that can solidify various hazardous wastes (Jinetal, 2016). Compared with the production of ordinary Portland cement, the synthesis of geopolymers requires lower energy and produces less carbon dioxide emissions (McLellanetal, 2011). There are many prospective studies on the use of geopolymers to stabilize heavy metals (El-Eswed et al., 2017; El-Eswed et al., 2015). Some scholars pay special attention to the development of industrial raw materials such as bottom ash (BocaSantaetal, 2016) and fly ash from the incineration of municipal solid waste (Jinetal, 2016).
[0004] Through the above analysis, the problems and defects of the prior art are as follows:
[0005] (1) If the existing incineration and landfill methods are not handled properly, they can easily cause serious environmental pollution and secondary pollution. At high temperatures, hexavalent chromium can also be produced, causing poisoning.
[0006] (2) In the existing solidification method, the cement solidification body has poor acid resistance and high permeability, and the heavy metal chromium cannot be completely sealed in the solidification body. It is difficult to suppress the leaching of hexavalent chromium in the acidic environment, thus causing harm to the environment. Summary of the invention
[0007] In view of the problems existing in the prior art, the present invention provides an alkali-activated slag-tannery sludge solidifying agent based on RSM and a method for optimizing its mix ratio.
[0008] The present invention is achieved by providing an alkali-activated slag-tannery sludge solidifying agent material (Tannery sludge solidified product, TSSP) and a method for optimizing its mix ratio. The alkali-activated slag-tannery sludge solidifying agent material and the method for optimizing its mix ratio include:
[0009] The response surface method (RSM) was used to establish a regression model to study the effects of water-binder ratio, alkali activator modulus, alkali activator dosage and cementitious material ratio (referred to as activator-binder ratio) on the early and late strength of alkali-activated slag-tannery sludge solidified cementitious materials; the craving function was used to optimize the mix ratio of alkali-activated slag-tannery sludge solidified cementitious materials, and the optimization results were experimentally verified; the alkali-activated slag-tannery sludge solidified cementitious materials were physically and chemically characterized using XRD, SEM-EDS, NMR and other testing methods. X-ray diffractometer and SEM-EDS scanning electron microscope were used to explore the microscopic mechanism of TSSP. Combined with the macroscopic experimental results, a microscopic basis is provided for it. This is a pretreatment step for the sludge to be turned into a building material, so that its particle size can be mixed with slag as a cementitious material. It can be solidified in the solidified body as microparticles.
[0010] The specific process is:
[0011] Step 1: Select tannery sludge, pre-treat it, and prepare sludge gelling material. The preparation process is as follows: use a crusher to crush the sludge plate after filter pressure dehydration into particles, then use a wall breaking machine to run for 1 minute, pass through a 0.15mm sieve, and then dry it in an oven for 2 hours to obtain the pre-treated sludge material.
[0012] Step 2: Prepare the alkali activator required for the test ratio one day in advance and seal it to cool naturally. Weigh a certain amount of slag and tannery sludge powder according to the required mass ratio, pour it into a stirring pot and stir it slowly for about 60 seconds to make it completely evenly distributed.
[0013] Step 3: slowly inject the prepared alkali activator into the stirring pot (keep the stirring pot stirring slowly during this period), and then stir quickly for 60 seconds to fully mix;
[0014] Step 4: Pour the slurry into a triple mold with a size of 40mm×40mm×40mm, and use a cement mortar vibrating table to vibrate and put it into the mold to ensure that air is discharged when the slurry is put into the mold and to avoid premature setting of the cementitious material, which may cause the test block to be delaminated.
[0015] Step 5: Place the test block in natural curing for 24 hours, then remove the mold and place it in a constant temperature and humidity curing box to continue curing to the specified age, then use anhydrous ethanol to terminate hydration for microscopic testing. The compressive strength test method refers to the "Test Method for Cement Mortar Strength (ISO Method)" (GB / T17671-1999).
[0016] Furthermore, the experimental design of the alkali-activated slag-tannery sludge solidifying agent material and the method for optimizing its mix ratio includes:
[0017] First, select the alkali excitation modulus M and the excitation ratio R AB , water-cement ratio R WB Design the experiment as a ratio variable. Determine the three variables and the basic range of variation;
[0018] Then, the Box-Benhnken model in RSM was used for experimental design and data analysis. The single-factor significance test determined that the interval of M was 0.8-1.2, and the change of M was adjusted by adding NaOH and water to the water glass. AB The interval range is 18% to 24%, R WB The interval range is 0.35-0.39;
[0019] Finally, the alkali-activated slag-tannery sludge solidifying agent ratio is optimized by combining the desire function. Using the desire function, we can perform multi-party optimization based on the regression model we established earlier using RSM. Simple RSM can only obtain the best ratio for one result (28d compressive strength). Using the desire function, we can find an optimal ratio with higher 28d and 7d strengths. Single factor gradient analysis was performed on each factor with 7d compressive strength and 28d compressive strength as response values.
[0020] Furthermore, the base excitation modulus M is:
[0021] M = moles of SiO2 / moles of Na2O
[0022] The irradiation ratio R AB for:
[0023] R AB = alkali activated mass / cementitious material mass
[0024] The water-binder ratio R WB for:
[0025] R WB = water mass / cementitious material mass. n is the mole number in chemistry, and M refers to the ratio of the moles of silicon dioxide and sodium oxide in the alkaline activator. Generally speaking, the lower the modulus, the more hydroxide ions are produced by the hydrolysis of water glass, and the stronger the alkalinity.
[0026] Further, the specific process of the RSM method is:
[0027] Based on the three-factor significance test, the regression model was established using the RSM method, and multiple regression fitting was performed to obtain the quadratic polynomial regression equations of the 7d compressive strength Y1 and the 28d compressive strength Y2:
[0028] Y1=53.4+3.36A-0.60B-0.16C-0.2AB-1.925AC-0.49BC-1.06A 2 -4.64B 2 -3.42C 2 -2.27A 2 C
[0029] Y2=70.08+2.64A+1.32B+2.54C-1.16AB+0.26AC+2.58BC-5.13A 2 -6.04B 2 -7.91C 2 -2.95AB 2 A is the ratio of glue to irradiation, B is the modulus, and C is the ratio of water to glue.
[0030] Further, the specific process of the single factor gradual change analysis is:
[0031] The DesignExpert software was used to conduct a comprehensive analysis of the relationship between the compressive strength test value and the three variable factors using a variety of fitting models, including linear model, two-factor (2FI) model, quadratic model and cubic model; the probability P value, lack of fit P value and correlation coefficient R of each model were output. 2 Correction value and R 2 Predicted value.
[0032] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0033] (1) The alkali-activated slag-tannery sludge solidifying agent strength regression model established by the RSM method in the present invention has high accuracy and credibility. The correlation coefficient between the measured value and the predicted value of the 28d compressive strength reaches above 0.96 (good correlation), the coefficient of variation is less than 4.0% (small discreteness), the signal-to-noise ratio is higher than 10.0 (high model precision), and the lack-of-fit P value is less than 0.01 (very significant). When the activator modulus is 0.8-1.2, the activator-binder ratio is 18%-24%, and the water-binder ratio is 0.35-0.39, the 28d average compressive strength of the alkali-activated slag-tannery sludge solidifying agent can reach above 60MPa, among which the activator-binder ratio is 21%, the activator modulus is 1, and the water-binder ratio is 0.37, which is the best mix ratio. The 28-day compressive strength can reach above 70MPa, reaching the level of high-strength composite materials. Based on XRD patterns and SEM-EDS microscopic analysis, it was found that the alkali-activated slag-tannery sludge solidifier contains calcium chrome garnet, which can effectively solidify / stabilize the heavy metal ions in the tannery sludge and effectively avoid possible secondary pollution problems. It is an environmentally friendly material.
[0034] Alkali-activated slag-tannery sludge solidifier has the characteristics of high strength and stability. The parameters (or indicators) of the alkali-activated slag-tannery sludge solidifier material optimized and determined based on RSM are accurate, which has important reference value and guiding significance for the mix design of similar alkali-activated cementitious material systems.
[0035] (2) The present invention utilizes the tanning sludge generated in the process of treating tanning wastewater as a resource - the sludge is harmlessly stabilized and disposed of by using building materials, so that high-strength curing agent materials can be obtained, and heavy metals in the tanning sludge can be solidified. The prevention and control of secondary pollution and resource utilization of sludge are promoted, and carbon emissions are reduced, which is in line with the requirements of major national plans. By building sludge treatment and disposal facilities, improving the level of sludge disposal technology and equipment, limiting sludge landfill and gradually reducing its scale, and reducing the use of sludge incineration in large and medium-sized cities with limited land use, etc., it will help promote the national urban sludge harmless disposal rate to reach 90% by 2025.
[0036] (3) The expected benefits and commercial value of the technical solution of the present invention after transformation are:
[0037] The strength of the alkali-activated slag-tannery sludge solidifying agent of the present invention is higher than that of P.O52.5 grade cement. At present, the market price of P.O52.5 grade cement is about 410 yuan / t, and the cost of the alkali-activated slag-tannery sludge solidifying agent is about 330 yuan / t, which is about 20% lower in price, and has certain advantages in terms of cost. At the same time, the alkali-activated slag-tannery sludge solidifying agent can effectively solidify / stabilize heavy metals, and is a green and environmentally friendly building material. The slag and tannery sludge used in it are both industrial wastes, which are abundant in resources and low in price, and have great significance for promotion.
[0038] (4) The technical solution of the present invention fills the technical gap in the industry at home and abroad:
[0039] The alkali-activated slag-tannery sludge solidifying agent of the present invention can achieve a strength of more than 60MPa and effectively solidify heavy metals in tannery sludge, providing technical support for solving both the building material and ecological disposal of tannery sludge, and making up for the technical deficiencies in the field of resource utilization and harmless coordinated disposal of industrial sludge at home and abroad.
[0040] (5) Whether the technical solution of the present invention solves the technical problems that people have been eager to solve but have never been able to solve successfully:
[0041] At present, sludge solidified by cement-based solidifying agent is mainly used for landfill treatment, and the overall strength requirement of the solidified body after solidification is relatively low. The required age for solidification ranges from 7 days to 28 days. At the same time, the effect of solidifying heavy metals is not good, there is secondary pollution, insufficient ecological and environmental benefits, and it is difficult to directly utilize resources to make building materials such as unburned bricks, ceramsite and filter materials, etc., and the engineering application conditions are limited. If it is to be used as building materials, it needs to be roasted at high temperature or a large amount of cement is used to increase the strength and block pollutants, but how to get rid of the high cost, high energy consumption and secondary pollution is still a problem.
[0042] In addition, according to statistics, the global CO2 greenhouse gas surge and the increase in carbon emissions are closely related to cement production, so it is very meaningful to replace cement in the curing agent with a new gelling material to achieve the same or even better curing effect. The present invention proposes a new formula for a tanning sludge solidified body, which can have a high strength of more than 60MPa in 28 days without high-temperature calcination and can also solve the secondary pollution problem of heavy metal chromium in tanning sludge, effectively overcoming the difficulties of building materials and ecological disposal of tanning sludge. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a flow chart of an RSM-based alkali-activated slag-tannery sludge solidifying agent and a method for optimizing its proportion provided in an embodiment of the present invention;
[0044] Figure 2 is a schematic diagram of XRD phase analysis of slag provided by an embodiment of the present invention;
[0045] Figure 3 The effect of the modulus of the activator provided in the embodiment of the present invention on the compressive strength of TTSP;
[0046] Figure 4 The effect of the jelly-gel ratio on the TSSP compressive strength provided by the embodiment of the present invention;
[0047] Figure 5 It is the effect of water-binder ratio on TSSP compressive strength provided by the embodiment of the present invention;
[0048] Figure 6 It is the effect of water-binder ratio on TSSP compressive strength provided by the embodiment of the present invention;
[0049] Figure 7 1 is a schematic diagram of the response surface of the interaction between the activator-to-glue ratio and the activator modulus on the TSSP compressive strength provided by an embodiment of the present invention;
[0050] Figure 8 It is a schematic diagram of the response surface of the interaction between the irradiation-binder ratio and the water-binder ratio on the TSSP compressive strength provided by an embodiment of the present invention;
[0051] Fig. 9 1 is a schematic diagram of the response surface of the interaction between the activator modulus and the water-binder ratio on the TSSP compressive strength provided by an embodiment of the present invention;
[0052] Fig.10 It is a schematic diagram of the response surface of the interaction between the activator-glue ratio and the activator modulus on the TSSP28d compressive strength provided by an embodiment of the present invention;
[0053] Fig.11 It is a schematic diagram of the response surface of the interaction between the irradiation-binder ratio and the water-binder ratio on the TSSP28d compressive strength provided by an embodiment of the present invention;
[0054] Fig.12 It is a schematic diagram of the response surface of the interaction between the activator modulus and the water-binder ratio on the TSSP28d compressive strength provided by an embodiment of the present invention;
[0055] Fig.13 This is the influence curve of factors near the center point on the compressive strength of TSSP28d provided by the embodiment of the present invention. DETAILED DESCRIPTION
[0056] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0057] In order to enable those skilled in the art to fully understand how to implement the present invention in detail, this section is an explanatory embodiment that expands and describes the technical solution of the claims.
[0058] like Figure 1 As shown, the RSM-based alkali-activated slag-tannery sludge solidifying agent and the method for optimizing its proportion include:
[0059] Step 1: Select tanning sludge, perform sludge pretreatment, and prepare sludge gelling material. The preparation process is as follows: use a crusher to crush the sludge plate after filter pressure dehydration into particles, then use a wall breaking machine to run for 1 minute, pass through a 0.15 mm sieve, and then use an oven to dry for 2 hours to obtain the pretreated sludge material;
[0060] Step 2: Prepare the alkali activator required for the test ratio one day in advance and seal it to cool naturally. Weigh a certain amount of slag and tannery sludge powder according to the required mass ratio, pour it into a stirring pot and stir it slowly for about 60 seconds to make it completely evenly distributed.
[0061] Step 3: slowly inject the prepared alkali activator into the stirring pot (keep the stirring pot stirring slowly during this period), and then stir quickly for 60 seconds to fully mix;
[0062] Step 4: Pour the slurry into a triple mold with a size of 40mm×40mm×40mm, and use a cement mortar vibrating table to vibrate and put it into the mold to ensure that air is discharged when the slurry is put into the mold and to avoid premature setting of the cementitious material, which may lead to stratification of the test block;
[0063] Step 5: Place the test block in natural curing for 24 hours, then remove the mold and place it in a constant temperature and humidity curing box to continue curing to the age of 7d and 28d, then use anhydrous ethanol to terminate hydration for microscopic testing. The compressive strength test method refers to the "Test Method for Cement Mortar Strength (ISO Method)" (GB / T17671-1999).
[0064] Further, the tanning sludge in step 1 is taken from a tannery in Pingyu County, Zhumadian City, Henan Province;
[0065] The preparation process of the sludge gelling material is as follows: the sludge plate after filter pressure dehydration is crushed into particles by a crusher, and then a wall breaking machine is used for 1 minute, and the sludge plate is passed through a 0.15 mm sieve and then dried in an oven for 2 hours to obtain the granular material.
[0066] Appearance and microscopic morphology of tannery sludge Figure 3 The main chemical components are shown in Table 2. The sludge gelling material was prepared by crushing the sludge plate after filter pressure dehydration into particles using a crusher, then running a wall breaker for 1 min, passing through a 0.15 mm sieve, and then drying in an oven for 2 hours.
[0067] Table 2 Main chemical components of tannery sludge
[0068] Table 2 Chemical composition of Tannery Sludge
[0069]
[0070] (a)(b)
[0071] Table 1 Main chemical components of cementitious materials
[0072] Table 1 Main chemical composition of blinder
[0073]
[0074] Granulated blast furnace slag was obtained from Henan Zhengzhou Hengyuan New Materials Co., Ltd. and is S95 slag. In this study, the chemical composition of the slag was evaluated with reference to GB / T203-2008 "Physical and Chemical Blast Furnace Slag Used in Cement" to reflect the potential activation activity of the slag. The mass fraction is 2.15>1.2, which is a high-quality slag; the alkalinity coefficient is 1.21>1, which is an alkaline slag; the activity coefficient is 0.49>0.25, which is a highly active slag; the hydraulic coefficient is 2.31>1, indicating that the active components are relatively high. Therefore, according to the rating coefficient results, it can be seen that the blast furnace slag used in this study is excellent and highly active. Figure 2 This is the XRD phase analysis of slag, which shows that the crystals in the slag are mainly calcite, calcite, magnesia and calcite. This shows that the slag contains rich calcium oxide and silica-alumina minerals, which can be activated under the action of alkaline activators.
[0075] Furthermore, the experimental design of the RSM-based alkali-activated slag-tannery sludge solidifying agent and its mix ratio optimization method includes:
[0076] First, select the modulus M and the gel ratio R AB , water-cement ratio R WB Design the experiment as the ratio variable. Determine the three variables and the basic range of variation;
[0077] Then, the Box-Benhnken model in the RSM method was used for experimental design and data analysis. According to the single-factor significance test, it was determined that the interval range of M was 0.8-1.2, and the change of M was adjusted by adding NaOH and water to the water glass. AB The interval range of is 18% to 24%, and the interval range of RWB is 0.35-0.39;
[0078] Finally, the mix ratio of alkali-activated slag-tannery sludge solidified cementitious materials was optimized in combination with the craving function, and single factor gradient analysis was performed on each factor with 7d compressive strength and 28d compressive strength as response values.
[0079] Furthermore, the alkali excitation modulus is:
[0080] M = moles of SiO2 / moles of Na2O;
[0081] The irradiation ratio R AB for:
[0082] R AB = alkali-activated mass / mass of cementitious material;
[0083] The water-binder ratio RWB for:
[0084] R WB = water mass / cementitious material mass. n is the mole number in chemistry, and M refers to the ratio of the moles of silicon dioxide and sodium oxide in the alkaline activator. Generally speaking, the lower the modulus, the more hydroxide ions are produced by the hydrolysis of water glass, and the stronger the alkalinity.
[0085] Further, the specific process of the response surface analysis method is:
[0086] Based on the three-factor significance test, the response surface analysis method was used to establish a regression model and perform multivariate regression fitting. The quadratic polynomial regression equations of the 7d compressive strength (Y1) and 28d compressive strength (Y2) were obtained as follows:
[0087] Y1=53.4+3.36A-0.60B-0.16C-0.2AB-1.925AC-0.49BC-1.06A 2 -4.64B 2 -3.42C 2 -2.27A 2 C (1)
[0088] Y2=70.08+2.64A+1.32B+2.54C-1.16AB+0.26AC+2.58BC-5.13A 2 -6.04B 2 -7.91C 2 -2.95AB 2 (2)
[0089] Further, the specific process of the single factor gradual change analysis is:
[0090] The DesignExpert software was used to conduct a comprehensive analysis of the relationship between the compressive strength test value and the three variable factors using a variety of fitting models, including linear model, two-factor (2FI) model, quadratic model and cubic model; then the probability (P) value, lack of fit P value, correlation coefficient (R 2 ) correction value and R 2 Predicted value.
[0091] Table 2 shows the coding and level of the independent variable factors in the experimental design, with high, medium and low coding values represented by 1, 0 and -1 respectively. Table 3 shows the Box-Behnken experimental plan and results.
[0092] Table 2 Experimental independent variable factors and levels
[0093]
[0094] Table 3 Box-Behnken test plan and results
[0095]
[0096]
[0097] The embodiments of the present invention have achieved some positive effects during the development or use process, and indeed have great advantages over the prior art. The following content is described in conjunction with data, charts, etc. of the test process.
[0098] Depend on Figure 3 , Figure 4 , Figure 5 The results of the single factor test show that the modulus of the activator, the ratio of activator to binder and the water-binder ratio all have a great influence on the early mechanical properties of TSSP: as the modulus of the activator decreases, the compressive strength first increases and then tends to be flat. The lower the modulus, the stronger the alkalinity of the activator, and the better the depolymerization effect of the silicon and aluminum minerals in the slag, indicating that the modulus of 1 is the critical value for the depolymerization effect, and too much alkali will no longer enhance the depolymerization ability; with the increase of the activator ratio, the mechanical properties of TSSP increase year-on-year, and an inflection point appears when it reaches 22% and begins to decline, indicating that the activator ratio of 22% is relatively optimal; the early strength of TSSP decreases with the increase of the water-binder ratio. The dependent variable range of the response surface was selected based on the results of the three groups of single factor tests, and subsequent mix optimization tests based on RSM were carried out.
[0099] The measured and predicted values of the 7d and 28d compressive strength of the alkali activated slag-tannery sludge solidifying agent specimens were obtained according to the experimental design conditions in Table 1. As shown in Table 2, the measured values of the mechanical properties of the specimens are close to the predicted values.
[0100] Table 4 Measured and predicted values of TSSP mechanical properties
[0101]
[0102]
[0103] The results of comprehensive analysis of the relationship between the compressive strength test value and the three independent variable factors using DesignExpert software using multiple fitting models are shown in Table 4. In statistical analysis, the significance of hypothesis test (sequential) analysis and lack of fit test (lackoffit) analysis is represented by P. It is generally believed that P < 0.01 is very significant, 0.01 ≤ P ≤ 0.05 is significant, and P > 0.05 is not significant.
[0104] From Table 5-6, we can see that the P value of the quadratic polynomial model in the compressive strength model is the smallest and very significant, and its P value of the lack-of-fit test analysis is the largest, R2 Correction value and R 2 The same method was used to conduct a comprehensive analysis of the 28d flexural strength using multiple models. It was found that: when the 7d compressive strength was modeled using a quadratic polynomial model, P = 0.0004 < 0.01, and when the 28d compressive strength was modeled using a quadratic polynomial model, P = 0.0002 < 0.01, both were very significant; when the flexural strength was modeled using a quadratic polynomial model, P = 0.0004, which was very significant; the lack of fit P value was large, and R 2 The correction value and R2 prediction value are both the largest. Therefore, it is recommended to use the quadratic polynomial model to analyze the compressive strength development of alkali-activated slag-tannery sludge solidifier.
[0105] Table 5 Comprehensive analysis results of various models for compressive strength (7d)
[0106]
[0107] Table 6 Comprehensive analysis results of various models for compressive strength (28d)
[0108]
[0109] Table 7 shows the results of variance analysis of the regression equation. F is the significance test index, and DF is the degree of freedom. The larger the F value and the smaller the P value, the smaller the probability that the original hypothesis of the model is not true, the stronger the model significance, and the higher the simulation accuracy; the P value of the lack of fit item reflects the significance of the irrelevance between the test data and the model. When its value is less than 0.05, it indicates that the significance is high, otherwise it is low. It can be seen from Table 5 that the P values of the quadratic polynomial regression equations of 7d compressive strength and 28d compressive strength are 0.0001 and 0.0017, respectively, and the F values are 39. .84393 and 15.34849, both are significant, among which the d compressive strength is the most significant; among the three single factors A, B, and C, for the 7d compressive strength model, factor A is the most significant, and factor C has little influence, and the order of factors affecting the 7d compressive strength is A>B>C; for the 28d compressive strength, all three factors have a certain influence, among which factor C (water-binder ratio) has a greater influence, and the order is C>A>B. Table 5 also lists the AB, AC, BC, A 2 , B 2 and C 2 The F value, P value, etc. show the degree of influence of each quadratic term in the equation. The P values of the lack-of-fit terms are 0.4935 and 0.8404, respectively, both greater than 0.05. It can be seen that the lack-of-fit of the model is not significant and the error is small, indicating that this regression equation has a high degree of fit with the actual situation.
[0110] Table 7 Results of variance analysis of regression equation
[0111]
[0112] Table 8 shows the results of the model credibility test analysis. 2 and R 2 The closeness of the correction value can be used to verify the fit of the regression equation, R 2 The closer it is to 1, the 2 and R 2 The difference of the correction value is less than 0.2; at the same time, the smaller the coefficient of variation (CV) (less than 10%), the greater the signal-to-noise ratio (adeqprecision) is than 4, indicating that the test reliability and accuracy are higher; std.dev. is the standard deviation; Press is the sum of squares of the predicted residuals. As shown in Table 5, the correlation coefficient R between the predicted value and the measured value is 2 They are 0.9852, 0.9624, R 2 The correction values are 0.9604 and 0.8997, the coefficients of variation are 1.74% and 3.53%, and the signal-to-noise ratios are 18.51 and 10.36, respectively. This shows that the regression equations of formulas (1) and (2) have high credibility and accuracy, can meet the requirements of fitting the actual situation, and have strong reliability.
[0113] Table 8 Model credibility test analysis results
[0114]
[0115] The embodiment of the present invention also analyzes the response surface interaction, first of all, the influence of independent variable factors on the 7d compressive strength and their interaction.
[0116] By projecting the actual value line of the design factor into the design interval, the influence curve of different factors can be obtained, and then the influence degree of different factors on the response value can be intuitively obtained. The influence curve of factors near the center point on the 7d compressive strength is shown in the figure below: Figure 6 The activator-binder ratio has the greatest influence on the 7d compressive strength. With the increase of the activator, the 7d compressive strength increases almost linearly. The activator modulus and water-binder ratio also have a significant effect on the compressive strength. With the increase of the parameters, the 7d compressive strength increases first and then decreases, which is consistent with the results of the single factor test.
[0117] In the three-dimensional response diagram, the color change from blue to red indicates the change of the response value from small to large. The faster the change, the steeper the slope of the response surface. The contour map can be obtained by response surface projection. The center of the smallest circle is the maximum response value. The circle indicates that the interaction between factors is weak, and the ellipse indicates that the interaction between factors is strong [LIP Q, ZHOU LG, MOU Y, et al. Extraction optimization of polysaccharide from zanthoxylum bungeanum using R SM and its antioxidant activity [J]. International Journal of Biological Macromolecules, 2015, 72: 19-]. The interactive response surface of the activator-binder ratio and the activator modulus, the activator-binder ratio and the water-binder ratio, and the activator modulus and the water-binder ratio on the compressive strength is shown in the figure. Figure 7 , Figure 8 , Fig. 9 As shown in the figure, there is a good interaction between the various factors, and the interaction between the activator modulus and the water-binder ratio is slightly worse. The activator-binder ratio, activator modulus, and water-binder ratio all have the highest point on the response surface, indicating that the response value (7d compressive strength) has a maximum value within the test range.
[0118] Then, the influence of independent variable factors on 28d compressive strength and their interactions were analyzed, including:
[0119] The interactive response surface of the three factors of activator-binder ratio and activator modulus, activator-binder ratio and water-binder ratio, activator modulus, and activator modulus and water-binder ratio on the 28d compressive strength is as follows: Figure 10 to Figure 12 The influence curve of factors near the center point on the 28d compressive strength is shown in Fig.13 As shown by Fig.13It can be seen that the activator-binder ratio, activator modulus, and water-binder ratio have a great influence on the 28d compressive strength. With the change of the activator modulus, the 28d compressive strength shows a trend of first increasing and then decreasing, and is optimal when the modulus is 1, which is consistent with the trend of 7d compressive strength, indicating that the modulus of 1 is suitable for the optimal ratio of AABS at all ages; with the increase of the activator-binder ratio, the 28d compressive strength first increases and then decreases. The reason is that the increase of the activator generates a large amount of CSH or CASH gel during the early hydration reaction, forming an isolation layer outside the slag, which hinders the hydration reaction of the slag in the isolation layer. With the increase of the water-cement ratio, a trend different from the 7d compressive strength appears. In the development trend of the 28d compressive strength, the strength of 0.37 is the largest and gradually decreases to both sides. This is because too low a water-cement ratio makes the concentration of alkali in the liquid phase relatively high in the early stage, making the reaction more violent and rapid, making it have higher strength at 7 days, but the disadvantage is that it is not conducive to the later strength development. Although the water-cement ratio of 0.37 is not as high as 0.35 at 7 days, its development is more stable, and the hydration is more complete, thus producing higher strength. Too high a water-cement ratio is not conducive to the development of the material. In addition, Fig.10 The medium-high line shows a circular trend, indicating that the interaction between the irradiation ratio and the water-binder ratio is poor. Fig.11 and Fig.12 The contour lines obtained by projecting the medium response surface show an elliptical trend, indicating that the interaction between the activator-binder ratio and the activator modulus, and between the activator modulus and the water-binder ratio is relatively good.
[0120] Finally, the optimal ratio is determined, including:
[0121] In the AASB mix optimization, compressive strength is taken as the optimization target, among which the 7d compressive strength and 28d compressive strength are both expected to be large characteristic response values, while ensuring the 28d compressive strength, as much as possible to meet the certain strength in the early stage. According to the above requirements, the AASB design optimization results were obtained using the Design-Expert software, as shown in Table 9. The test verification measured the 7d compressive strength of AASB to be 53.77 and the 28d compressive strength to be 70.71MPa, which are close to the model prediction values, indicating that the optimization mix method and the established model are reliable and have good predictive performance.
[0122] Table 9 Response surface optimization results (point prediction)
[0123]
[0124] From the above analysis, we can draw the following conclusions:
[0125] (1) With the increase of activator-binder ratio, the early compressive strength increases year-on-year, but too much activator is not conducive to the development of later compressive strength; with the increase of activator modulus, the compressive strength at 7d and 28d increases first and then decreases, and both have the best effect when the modulus is 1; with the increase of water-binder ratio, the compressive strength at 7d shows a downward trend, but the compressive strength at 28d shows an upward trend and then downward trend, and reaches the maximum value when the water-binder ratio is 0.37.
[0126] (2) According to the response surface analysis, the three parameters have significant effects on the compressive strength in the early and late stages. For the early strength, the interaction of the three factors is good. For the 28d compressive strength, the interaction between the activator modulus and the activator-binder ratio is poor, and the contour map is circular; the interaction between the activator-binder ratio and the water-binder ratio, and the activator modulus and the water-binder ratio are general. The highest point appears on the interaction surface of the three factors, indicating that the response value has a maximum value within the range.
[0127] (3) The optimal ratio was obtained by using the model equation obtained by response surface analysis: the activator-binder ratio was 21%, the activator modulus was 1.0, and the water-binder ratio was 0.37. The actual value had a small deviation from the model predicted value, which proved that the response surface analysis was accurate in determining the parameters in the optimal combination. It has important reference value and guiding significance for the mix design of alkali-activated cementitious material system, and proved that the use of response surface for multi-index optimization is a very feasible method for AASB mix design.
[0128] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. An alkali-activated slag-tannery sludge solidifying agent based on RSM and a method for optimizing its proportion, characterized in that: The RSM-based alkali-activated slag-tannery sludge solidifying agent and the method for optimizing its proportion include: The response surface method (RSM) was used to establish a regression model to study the effects of water-binder ratio, alkali activator modulus, and alkali activator dosage on the early and late strengths of alkali-activated slag-tannery sludge solidified cementitious materials. The mix ratio of alkali-activated slag-tannery sludge solidified cementitious materials was optimized in combination with the desire function, and the optimization results were experimentally verified. The alkali-activated slag-tannery sludge solidified cementitious materials were physically and chemically characterized using X-ray diffractometer (XRD), scanning electron microscope-energy dispersive spectrometer (SEM-EDS), and nuclear magnetic resonance (NMR). The specific process of the RSM-based alkali-activated slag-tannery sludge solidifying agent and the method for optimizing its proportion is as follows: Step 1, selecting tanning sludge to prepare sludge gelling material; Step 2: Prepare the alkali activator required for the test ratio one day in advance and seal it to cool naturally. Weigh a certain amount of slag and tannery sludge powder according to the required mass ratio, pour it into a stirring pot and stir it slowly for about 60 seconds to make it completely evenly distributed. Step 3: slowly inject the prepared alkaline activator into the stirring pot, keep stirring the stirring pot slowly during the injection, and stir quickly for 60 seconds after injection to fully mix it; Step 4: Pour the slurry into a triple mold with a size of 40 mm × 40 mm × 40 mm, and use a cement mortar vibrating table to vibrate and put the slurry into the mold to ensure that air is discharged when the slurry is put into the mold and to avoid premature setting of the cementitious material, which may lead to stratification of the test block. Step 5: After the test block is placed in natural curing for 24 hours, the mold is removed and placed in a constant temperature and humidity curing box for continued curing to 7 days and 28 days. Then, anhydrous ethanol is used to terminate the hydration for microscopic testing and compressive strength testing; The tanning sludge in the step 1 is taken from a tannery in Pingyu County, Zhumadian City, Henan Province; The preparation process of the sludge gelling material is as follows: using a crusher to crush the sludge plate after filter pressure dehydration into particles, and then using a wall breaking machine to run for 1 minute, passing through a 0.15mm sieve, and then drying in an oven for 2 hours to obtain; The experimental design of the RSM-based alkali-activated slag-tannery sludge solidifying agent and its mix ratio optimization method includes: First, select the modulus M and the gel ratio R AB , water-cement ratio R WB Design the experiment as the ratio variable. Determine the three variables and the basic range of variation; Then, the Box-Benhnken model in the response surface analysis method was used for experimental design and data analysis. According to the single factor significance test, it was determined that the interval range of M was 0.8-1.2, and the change of M was adjusted by adding NaOH and water to the water glass. AB The range of is 18% to 24%, and the range of RWB is 0.35-0.39; the average compressive strength of the alkali-activated slag-tannery sludge solidified material prepared within this range reaches more than 60MPa at 28 days; Finally, the mix ratio of alkali-activated slag-tannery sludge solidified cementitious materials was optimized, and single factor gradient analysis was performed on each factor with 7d compressive strength and 28d compressive strength as response values.
2. The RSM-based alkali-activated slag-tanning sludge solidifying agent and its mix ratio optimization method as claimed in claim 1, characterized in that: The alkali excitation modulus: M = moles of SiO2 / moles of Na2O The irradiation ratio R AB for: R AB = alkali activated mass / cementitious material mass The water-binder ratio R WB for: R WB = Water mass / cementitious material mass.
3. The RSM-based alkali-activated slag-tanning sludge solidifying agent and its mix ratio optimization method as claimed in claim 1, characterized in that: The specific process of the response surface analysis method is as follows: Based on the single factor gradual change analysis, the response surface analysis method was used to establish a regression model, and multiple regression fitting was performed to obtain the 7d compressive strength. Y 1 and 28d compressive strength Y The quadratic polynomial regression equation for 2 is: 。 4. The RSM-based alkali-activated slag-tannery sludge solidifying agent and its mix ratio optimization method as claimed in claim 1, characterized in that: The specific process of the single factor gradual change analysis is: Design Expert software was used to conduct a comprehensive analysis of the relationship between the compressive strength test value and the three variable factors using a variety of fitting models, including linear model, two-factor 2FI model, quadratic model and cubic model; the probability P value, lack of fit P value and correlation coefficient R of each model were output. 2 Correction value and R 2 Predicted value.
Citation Information
Cited By