Inkjet ink, method for producing printed matter, and printed matter

By using scaly metal particles with an average long diameter of less than 400nm and surface modification technology in inkjet inks, combined with photocationic or radical polymerization, the problem of satellite droplets is solved, and high metallic gloss and durability of printed matter are improved.

CN116075433BActive Publication Date: 2024-10-08NATOCO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180055138.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-08
Filing Date
2021-07-13
Publication Date
2024-10-08
Estimated Expiration
2041-07-13

AI Technical Summary

Technical Problem

Existing inkjet inks tend to produce satellite droplets when improving metallic gloss, and it is difficult to achieve good metallic gloss and reduction of satellite droplets at the same time.

Method used

Use scaly metal particles with an average long diameter of less than 400nm, with a content of 2 to 10% by mass, and optimize the composition of the inkjet ink through surface modification and appropriate polymerization methods (such as photocationic or free radical polymerization) to improve the aggregation of the ink. properties and solidification.

Benefits of technology

It effectively suppresses the generation of satellite droplets, while achieving high metallic gloss printing, improving the durability of the printing and maintaining the metallic gloss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116075433B_ABST
    Figure CN116075433B_ABST
Patent Text Reader

Abstract

An inkjet ink comprising flaky metal particles. The average major diameter of the flaky metal particles is 400 nm or less (preferably 50 to 200 nm). In addition, the inkjet ink comprises 2 to 10% by mass of flaky metal particles. The flaky metal particles preferably contain indium and / or chromium. The inkjet ink may be a free radical polymerization type or a cationic polymerization type.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an inkjet ink, a method for producing a printed article, and a printed article. More specifically, it relates to an inkjet ink containing scaly metal particles, a method for producing a printed article using the inkjet ink, and a printed article comprising a cured product of the inkjet ink. Background Art

[0002] The use of inkjet technology to draw metallic images on the surface of objects was studied.

[0003] Hot stamping has traditionally been the mainstream method for creating metallic images on the surface of objects. However, hot stamping can be complex and unsuitable for high-volume, low-volume production. Consequently, research is underway to create metallic images on the surface of objects using the relatively simple inkjet method, which is well-suited for high-volume, low-volume production.

[0004] Patent Document 1 describes a UV-curable inkjet ink composition containing an aluminum pigment, phenoxyethyl (meth)acrylate, and ricinoleic acid triglyceride phosphate. The composition contains ricinoleic acid triglyceride phosphate in an amount of 0.05% to 5% by mass relative to the total mass of the ink composition. Furthermore, the aluminum pigment in the composition is in the form of flat particles having an average thickness of 5 nm to 30 nm and a 50% average particle size of 0.5 μm to 3 μm.

[0005] Patent Document 2 describes an ink composition characterized by containing (component A) aluminum flaky metal particles, (component B) a cationically polymerizable compound, and (component C) a photocationic polymerization initiator, wherein the polyfunctional monomer accounts for 15 to 99.9% by weight of component B.

[0006] Patent Document 3 describes an active energy ray-curable ink composition comprising at least (A) flaky metal particles, (B) a polymerizable compound, and (C) a photopolymerization initiator. This active energy ray-curable ink composition has an L* value of 30 or greater at the liquid interface. Furthermore, the flaky metal particles (A) have a 50% volume average diameter of 0.05 to less than 0.5 μm, an average thickness of 5.0 to less than 50.0 nm, and an aspect ratio (50% volume average diameter / average thickness) of 4 to 50.

[0007] Patent Document 4 describes an image forming method comprising a white ink applying step of applying a white ink containing a metal oxide having a number average diameter of 200 nm to 700 nm and a polymer to a recording medium, and a glitter ink applying step of applying a glitter ink containing a glitter pigment to the area on the recording medium to which the white ink has been applied. The volume Vp of the metal oxide in the white ink and the volume Ve of the polymer in the white ink satisfy 0.6 ≤ Vp / (Vp + Ve).

[0008] Patent Document 5 describes an image-formed article comprising a substrate, a base layer formed on the substrate surface, and an ink layer formed in contact with the base layer. The ink layer is a collection of multiple dots containing metal nanoparticles and has a thickness of 100 nm or more.

[0009] Patent Document 6 describes an edible ink containing polyvinyl pyrrolidone and silver.

[0010] Patent Document 7 describes a glitter inkjet ink containing metal nanoparticles, a dispersant adsorbed on the surface of the metal nanoparticles, emulsion resin particles, and a solvent. Here, assuming the average particle size of the metal nanoparticles is D1 and the average particle size of the emulsion resin particles is D2, the relationship 0.05 < D2 / D1 < 1 is satisfied.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 2012-102295

[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 2012-46577

[0015] Patent Document 3: Japanese Patent No. 6672432

[0016] Patent Document 4: Japanese Patent Application Publication No. 2019-155598

[0017] Patent Document 5: Japanese Patent Application Publication No. 2019-162741

[0018] Patent Document 6: Japanese Patent Application Laid-Open No. 2020-2338

[0019] Patent Document 7: International Publication No. 2018 / 181080 Summary of the Invention

[0020] Problems to be solved by the invention

[0021] As described above, various studies have been conducted on providing an image having a metallic luster on the surface of an article by an inkjet method.

[0022] However, while developing inkjet inks containing flaky metal particles, the inventors discovered that increasing the concentration of flaky metal particles to enhance the metallic gloss of printed images tends to result in the generation of satellite droplets. Specifically, preliminary research by the inventors revealed that the generation of satellite droplets is inversely proportional to the metallic gloss of the printed image.

[0023] The present invention has been made in view of the above circumstances, and one object of the present invention is to provide an inkjet ink that is less likely to generate satellite droplets and can form an image with high metallic gloss.

[0024] Means for solving problems

[0025] The inventors of the present application have completed the invention provided below and solved the above-mentioned problems.

[0026] According to the present invention,

[0027] Provided is an inkjet ink comprising scaly metal particles.

[0028] The average major diameter of the flaky metal particles is 400 nm or less.

[0029] The inkjet ink contains 2 to 10% by mass of the flaky metal particles.

[0030] In addition, according to the present invention, there is provided a method for producing a printed matter, comprising:

[0031] An image forming step of discharging the inkjet ink onto a substrate surface to form an image; and

[0032] A curing step of curing the discharged inkjet ink.

[0033] Furthermore, according to the present invention, there is provided a printed article comprising a cured product of the inkjet ink.

[0034] Effects of the Invention

[0035] According to the present invention, it is possible to provide an inkjet ink that is less likely to generate satellite droplets and that can form an image having a high metallic gloss. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] [ Figure 1 ] is a reference diagram for illustrating the evaluation method of satellite droplets in the embodiment. DETAILED DESCRIPTION

[0037] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0038] The drawings are for illustration purposes only, and the shapes, dimensional ratios, etc. of the components in the drawings do not necessarily correspond to actual products.

[0039] In this specification, the expression "X to Y" in describing a numerical range means not less than X and not more than Y unless otherwise specified. For example, "1 to 5 mass %" means "1 mass % or more and 5 mass % or less."

[0040] In the description of a group (atomic group) in this specification, the description without specifying whether it is substituted or unsubstituted includes both groups with no substituents and groups with substituents. For example, "alkyl" includes not only alkyl groups with no substituents (unsubstituted alkyl groups) but also alkyl groups with substituents (substituted alkyl groups).

[0041] The term "(meth)acrylic-" in this specification encompasses both acrylic- and methacrylic-. The same applies to similar terms such as "(meth)acrylate." The term "organic group" in this specification, unless otherwise specified, refers to an atomic group formed by removing one or more hydrogen atoms from an organic compound. For example, a "monovalent organic group" refers to an atomic group formed by removing one hydrogen atom from any organic compound.

[0042] <Inkjet Ink>

[0043] The inkjet ink of this embodiment contains scaly metal particles.

[0044] The average major diameter of the scaly metal particles is 400 nm or less.

[0045] The scaly metal particles are contained in the inkjet ink in an amount of 2 to 10% by mass.

[0046] As mentioned above, increasing the concentration of metallic pigments to enhance metallic gloss has traditionally resulted in the formation of satellite droplets, making it difficult to simultaneously achieve good metallic gloss and reduce satellite droplets. This is presumably because increasing pigment concentration tends to break the ligament (the tail-like portion that forms behind a droplet ejected from an inkjet head). Specifically, higher pigment concentrations impair the ink's "matomari" (aggregation) properties, resulting in an increase in small droplets (i.e., satellite droplets) that are not absorbed by the main droplet.

[0047] In particular, when flaky metal particles are used as pigments to achieve a metallic luster, their unique "scaly" shape significantly affects the ink's "aggregation" and "flow properties" compared to spherical particles. Therefore, it is speculated that the use of flaky metal particles is more likely to produce satellite droplets.

[0048] Based on the above, this embodiment uses flaky metal particles with an average major diameter of 400 nm or less. Using relatively small flaky metal particles with an average major diameter of 400 nm or less improves ink aggregation, making satellite droplets less likely to form. Therefore, even at a flaky metal particle concentration of 2 to 10% by mass, satellite droplets are less likely to form. Furthermore, since a relatively large amount of flaky metal particles can be used, printed materials with a superior metallic luster can be produced.

[0049] In addition, in the present embodiment, by making the metal particles "scaly," metallic luster can be easily obtained (compared to spherical metal particles of the same amount).

[0050] It should be noted that, according to the inventors of this application, even when using "relatively small" flaky metal particles with an average major diameter of 400 nm or less, a printed material with sufficient metallic luster can be obtained when a sufficient amount of flaky metal particles such as 2 to 10 mass % is contained in the inkjet ink.

[0051] Hereinafter, the components contained, physical properties, etc. of the inkjet ink according to this embodiment will be described in detail.

[0052] (Flake-like metal particles)

[0053] The inkjet ink of this embodiment contains flaky metal particles. "Flake" refers to a concept encompassing shapes such as flat plates and curved plates. Specifically, it refers to a shape whose area when viewed from a particular direction (when viewed from above) is larger than when viewed from a direction perpendicular to that direction.

[0054] In the flaky metal particles, the aspect ratio determined by calculation of (average major diameter / average thickness) is preferably 2 or greater, more preferably 2.5 or greater, even more preferably 3 or greater, and particularly preferably 3.5 or greater. The upper limit of the aspect ratio is not particularly limited, but is, for example, 100 or less, preferably 75 or less, more preferably 50 or less, and particularly preferably 25 or less.

[0055] The average major diameter of the flaky metal particles may be 400 nm or less, preferably 50 to 400 nm, more preferably 50 to 350 nm, further preferably 50 to 200 nm, and particularly preferably 100 to 200 nm. Using flaky metal particles with a smaller average major diameter can further suppress the formation of satellite droplets.

[0056] The average thickness of the scaly metal particles is preferably 10 to 50 nm, more preferably 20 to 40 nm.

[0057] The “average major diameter” can be determined by photographing the scaly metal particles using an electron microscope and averaging the major diameters of 50 random scaly metal particles in the photographed image. The same applies to the “average thickness”.

[0058] By using scaly metal particles having an appropriate average major diameter, average thickness, or aspect ratio, the metallic gloss of the final printed material can be further improved while maintaining inkjet performance (eg, dischargeability).

[0059] The scaly metal particles may contain one or more metals such as indium, chromium, silver, and aluminum, and preferably contain indium and / or chromium.

[0060] The flaky metal particles of indium and / or chromium have an advantage in that flaky metal particles having an average major diameter and an average thickness within the above range can be easily obtained.

[0061] Furthermore, the inventors of the present application have discovered that, compared to conventionally used aluminum pigments, indium and / or chromium are less likely to interact with curable components in inkjet inks and less likely to induce a curing reaction, thereby easily improving the storage stability of the ink before use.

[0062] Furthermore, indium and / or chromium do not significantly inhibit the curing reaction of the inkjet ink, and therefore it is easy to achieve both the curability (curing speed) of the ink and the storage stability before use.

[0063] Furthermore, indium and chromium are less likely to undergo chemical changes (oxidation, corrosion, etc.) in inkjet inks or their cured products than conventional aluminum pigments, and therefore are more likely to maintain the metallic gloss of the formed image.

[0064] From the perspective of brightness, at least a portion of the flaky metal particles is usually not a compound such as an oxide, nitride, or hydroxide, but rather a simple metal. For example, the above-mentioned indium and / or chromium are preferably metallic indium and / or metallic chromium. However, this does not mean that the flaky metal particles are completely free of compounds such as oxides, nitrides, and hydroxides. As long as they have brightness and / or metallic luster, a portion (not all) of the flaky metal particles may also be an oxide, nitride, hydroxide, etc. In addition, the flaky metal particles may also be an alloy.

[0065] The average particle size of the scaly metal particles determined by a light scattering method is not particularly limited and can be appropriately selected in consideration of desired metallic gloss, ease of ink discharge, and the like.

[0066] The Z-average particle size of the flaky metal particles is preferably 50 to 500 nm, more preferably 100 to 400 nm. By increasing the Z-average particle size to a certain extent, the metallic gloss of the final image can be further enhanced. Furthermore, by not excessively increasing the Z-average particle size, the inkjet ink tends to be discharged more smoothly from the nozzle. This is also believed to prevent nozzle clogging.

[0067] The Z-average particle size of the flaky metal particles can be measured by a light scattering method in accordance with ISO 22142: 2017. More specifically, the Z-average particle size can be determined by using a cumulant method to determine the harmonic mean particle size weighted by the scattered light intensity.

[0068] An example of a measuring device capable of measuring using the light scattering method is the Zetasizer Nano ZS manufactured by Malvern. The measurement is generally performed in a wet format, that is, a sample prepared by dispersing scaly metal particles in a solvent can be used as the measurement sample.

[0069] The surface of the flaky metal particles can be modified through physical or chemical treatment. This modification can sometimes be expected to inhibit metal oxidation, preventing loss of metallic luster. Furthermore, / or, modification can localize the flaky metal particles to the upper portion of the cured film, further enhancing metallic luster.

[0070] In one embodiment, the surface of the flaky metal particles is preferably modified with a group containing a linear or branched alkyl group having 4 or more carbon atoms (specifically, 4 to 230 carbon atoms), a silicon-containing group, or a fluorine-containing group (collectively referred to as "specific functional groups"). The presence of at least one of these specific functional groups on the surface of the flaky metal particles suppresses sedimentation of the flaky metal particles during the uncured stage after the inkjet ink is dropped onto the substrate surface (this can be explained by theories such as thermodynamics and surface energy). As a result, the metallic gloss of the final image can be further enhanced.

[0071] Particularly when using flaky metal particles having a large specific gravity (for example, when using indium particles or chromium particles), modifying the surface of the flaky metal particles to suppress sedimentation of the flaky metal particles can improve the metallic gloss of the final image.

[0072] More specifically, the surface of the scaly metal particles is preferably modified with a group containing a structure represented by the following general formula (1).

[0073] [Chemical Formula 1]

[0074]

[0075] In the general formula (1),

[0076] The two Rs are independently a hydrogen atom, a monovalent organic group or a group represented by the following general formula (2), and at least one of the two Rs is a group represented by the following general formula (2).

[0077] L is a divalent linking group,

[0078] * is the bond connecting to other chemical structures.

[0079] [Chemical Formula 2]

[0080] *-CH2-CHR 2 -COOR 1 (2)

[0081] In the general formula (2),

[0082] R 1 is a group containing a linear or branched alkyl group having 4 or more carbon atoms, a group containing a silicon atom, or a group containing a fluorine atom,

[0083] R 2 is a hydrogen atom or a methyl group.

[0084] In the general formula (1), when R is not a group represented by the general formula (2), R is a hydrogen atom or a monovalent organic group. Examples of the monovalent organic group include alkyl, cycloalkyl, alkoxy, aryl, aralkyl, alkylcarbonyl, alkoxycarbonyl, and alkylcarbonyloxy groups.

[0085] The number of carbon atoms in the monovalent organic group is not particularly limited, and is, for example, 1 to 20, specifically 1 to 10.

[0086] From the viewpoint of further suppressing the sedimentation of the flaky metal particles, R is preferably a group containing a linear or branched alkyl group having 4 or more carbon atoms, and more preferably a linear or branched alkyl group having 4 or more carbon atoms.

[0087] From the viewpoint of further suppressing the sedimentation of the flaky metal particles, it is preferred that both of the two Rs in the general formula (1) are groups represented by the general formula (2).

[0088] In the general formula (1), examples of the divalent linking group of L include an alkylene group (which may be linear or branched), an alicyclic group (which may be monocyclic or polycyclic), an aromatic group, an ether group, an ester group, a thioether group, a sulfide group, a carbonyl group, an amide group (-CONH-), an -NH- group, and a group formed by linking two or more of them.

[0089] The total number of carbon atoms in L is not particularly limited. For example, when L is an alkylene group, the preferred number of carbon atoms is 1 to 12, and more preferably 1 to 6. When L is an alicyclic group, the preferred number of carbon atoms is 3 to 12. When L is an aromatic group, the preferred number of carbon atoms is 6 to 20.

[0090] L is preferably (i) an alkylene group, or (ii) a group formed by linking an alkylene group to at least one group selected from the group consisting of an ether group, an ester group, a thioether group, a sulfide group, a carbonyl group, a -NH- group, and an amide group (-CONH-).

[0091] In the general formula (2), R 1 In the case of a linear or branched alkyl group having 4 or more carbon atoms, examples of the alkyl group include n-butyl, isobutyl, pentyl, neopentyl, isopentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, isolauryl, isostearyl, isocetyl, octyldodecyl, myristyl, 2-ethylhexyl, 2-hexyldecyl, 2-decylmyristyl, 2,7-dimethylhexadecyl, isotridecyl, 2,2-dimethyllauryl, 2,3-dimethyllauryl, 2,2-dimethylstearyl, and 2,3-dimethylstearyl. Of course, the alkyl group is not limited to these.

[0092] From the perspective of raw material availability and ease of manufacturing, R 1 Preferably, it is a linear or branched alkyl group having 4 or more carbon atoms (R 1 It is not a group containing an alkyl group as a part of the structure, but R 1 As a whole, it is represented by the alkyl group on the left).

[0093] In the general formula (2), R 1 When it is a group containing silicon atoms, as R 1 Examples thereof include a group containing an alkylsilyl group, a group containing a polysiloxane structure, a group containing a cyclic siloxane structure, and a group containing a silsesquioxane (ladder type, cage type) structure.

[0094] Among them, a group containing an alkylsilyl group or a group containing a polysiloxane structure is preferred due to the ease of obtaining the raw materials. More specifically, preferred examples of the polysiloxane structure include polydialkylsiloxane structures such as a polydimethylsiloxane structure (-Si(CH3)2-O-), and a polydiphenylsiloxane structure (-Si(C6H5)2-O-).

[0095] In the general formula (2), as R 1Specific examples of the group containing a fluorine atom include fluorine-substituted alkyl groups, fluorine-substituted cycloalkyl groups, fluorine-substituted alkoxy groups, fluorine-substituted aryl groups, fluorine-substituted aralkyl groups, fluorine-substituted alkylcarbonyl groups, fluorine-substituted alkoxycarbonyl groups, and fluorine-substituted alkylcarbonyloxy groups.

[0096] R 1 The fluorine-containing group may be a group in which all hydrogen atoms are replaced by fluorine atoms (perfluorinated group) or a group in which only a part of the hydrogen atoms are replaced by fluorine atoms. 1 In the fluorine-containing group, it is preferred that 50 mol % or more of the hydrogen atoms are substituted with fluorine atoms.

[0097] Based on the factors such as the difficulty in sedimentation and compatibility with other ingredients in the preparation of inkjet ink, R 1 A group containing a branched alkyl group or a group containing a polydimethylsiloxane structure is preferred.

[0098] The method for modifying the surface of the scaly metal particles is not particularly limited. For example, when modifying the surface with a group represented by the general formula (1), the following first and second steps can be used.

[0099] ·First process

[0100] First, raw material flaky metal particles (referred to as "raw material particles" in the chemical formula below) are reacted with a silane coupling agent represented by the following general formula (1a) to introduce -NH2 structures onto the surfaces of the flaky metal particles. Specific examples of the silane coupling agent include the aminosilanes listed below under "Other Components."

[0101] [Chemical Formula 3]

[0102]

[0103] In the general formula (1a),

[0104] R 3 When there are multiple groups, each group is independently an alkyl group or an acyl group.

[0105] R 4 When there are multiple groups, each group is independently an alkyl group.

[0106] m is an integer from 1 to 3, n is an integer from 0 to 2, m+n is 3,

[0107] L is a divalent linking group.

[0108] R 3 The number of carbon atoms in is preferably 1-10, more preferably 1-4.

[0109] As R 3Specific examples include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, and decyl, and acyl groups represented by -CO-R' (R' is, for example, any of the alkyl groups listed here).

[0110] As R 3 , preferably methyl or ethyl, particularly preferably methyl.

[0111] R 4 The number of carbon atoms in is preferably 1-10, more preferably 1-4.

[0112] As R 4 Specific examples of R include 3 The alkyl group is exemplified as follows.

[0113] As R 4 , preferably methyl or ethyl, particularly preferably methyl.

[0114] m is preferably 2 or 3, more preferably 3.

[0115] n is preferably 0 or 1, more preferably 0.

[0116] Specific examples of the divalent linking group of L are the same as those of L in the general formula (1).

[0117] Second process

[0118] A compound having a specific functional group is bonded to -NH2 introduced onto the surface of the raw material scaly metal particles. More specifically, a compound represented by the following general formula (2a) is Michael-added to -NH2 introduced onto the surface of the raw material particles. This allows the carbon-carbon double bond of the compound represented by general formula (2a) to react with -NH2 and bond.

[0119] [Chemical Formula 4]

[0120] CH2=CHR 2 -COOR 1 (2a)

[0121] R in the general formula (2a) 1 and R 2 The definition and specific examples of are the same as those of general formula (2).

[0122] In the second step, by adjusting the amount of the compound represented by general formula (2a), scaly metal particles can be obtained in which one or both of the R groups in general formula (1) are modified with groups represented by general formula (2). In principle, by reacting 2 moles or more of the compound represented by general formula (2a) with 1 mole of -NH2, filler particles can be obtained in which both of the R groups in general formula (1) are groups represented by general formula (2).

[0123] In the above, the scaly metal particles as a raw material are reacted with the silane coupling agent represented by the general formula (1a) in the first step, and Michael addition is performed on the compound represented by the general formula (2a) in the second step.

[0124] Alternatively, the scaly metal particles may be surface-modified by (i) first reacting a silane coupling agent represented by the general formula (1a) with a compound represented by the general formula (2a), and (ii) then reacting the reaction product obtained in (i) with the raw material scaly metal particles.

[0125] While the surface modification of the flaky metal particles has been described above, it should be noted that unmodified flaky metal particles can also be used in the inkjet ink of this embodiment. Using unmodified flaky metal particles can reduce manufacturing costs, for example.

[0126] Flaky metal particles (flaky metal particles whose surfaces are not modified with specific functional groups) can be obtained, for example, from Oike Industries Co., Ltd. For methods of producing flaky metal particles, reference can also be made to Japanese Patent Application Laid-Open Nos. 11-323223, 11-343436, and 2011-52041.

[0127] The inkjet ink of the present embodiment may contain only one type of flaky metal particles, or may contain two or more types of flaky metal particles.

[0128] Furthermore, the inkjet ink of this embodiment may contain, for example, a pigment different from the flaky metal particles (non-flaky metal particles, etc.) within a range that does not excessively impair performance. Of course, the inkjet ink of this embodiment may not contain such a pigment.

[0129] The ratio of flaky metal particles in the inkjet ink of this embodiment can be 2 to 10% by mass, more preferably 2 to 6% by mass, relative to the total inkjet ink. By setting this ratio to 2% or more, a sufficient metallic luster can be achieved in the final printed material. Furthermore, by setting this ratio to 10% or less, a sufficient amount of other components (curable components) can be included in the inkjet ink. This is preferable for reducing nozzle clogging and improving the durability of the final printed material.

[0130] (Regarding the polymerization method and curable components of inkjet inks)

[0131] The inkjet ink of the present embodiment is typically photocurable or thermosetting, and is preferably photocurable.

[0132] The polymerization method of the inkjet ink is not particularly limited. The polymerization method is preferably cationic polymerization or free radical polymerization. Specifically, the inkjet ink of this embodiment may include (i) an inkjet ink containing a cationically polymerizable compound and a cationic polymerization initiator in addition to flaky metal particles, or (ii) an inkjet ink containing a free radical polymerizable compound and a free radical polymerization initiator in addition to flaky metal particles.

[0133] Hereinafter, the cationically polymerizable compound and the cationic polymerization initiator in (i) and the radically polymerizable compound and the radical polymerization initiator in (ii) will be described.

[0134] First, the cationically polymerizable compound and the cationic polymerization initiator in the above (i) will be described.

[0135] Cationic polymerizable compounds

[0136] Typical examples of cationically polymerizable compounds include oxetane compounds, epoxy compounds, and vinyl ether compounds. Two or more of these compounds may be used in combination. For example, a cationically polymerizable ink may contain both an oxetane compound and an epoxy compound. By using two or more different cationically polymerizable compounds in combination, both curability and storage stability can be achieved at higher levels.

[0137] In the present embodiment, it is particularly preferred that the cationically polymerizable compound include a compound having an epoxy group and / or an oxetanyl group.

[0138] Examples of epoxy compounds include aromatic epoxides, alicyclic epoxides, and aliphatic epoxides. Examples of aromatic epoxides include diglycidyl ethers or polyglycidyl ethers obtained by reacting a polyphenol having at least one aromatic ring or its alkylene oxide adduct with epichlorohydrin. Examples include diglycidyl ethers or polyglycidyl ethers of bisphenol A or its alkylene oxide adducts, diglycidyl ethers or polyglycidyl ethers of hydrogenated bisphenol A or its alkylene oxide adducts, and Novolac epoxy resins. Examples of alkylene oxides include ethylene oxide and propylene oxide.

[0139] As the epoxy compound, a compound having two or more epoxy groups in one molecule is preferred, and a compound having 2 to 6 epoxy groups in one molecule is more preferred.

[0140] As the alicyclic epoxide, a compound containing cyclohexene oxide or cyclopentene oxide obtained by epoxidizing a compound having at least one cyclic hydrocarbon ring such as a cyclohexene ring or a cyclopentene ring with an oxidizing agent such as hydrogen peroxide or a peracid can be used.

[0141] As the aliphatic epoxide, diglycidyl ethers or polyglycidyl ethers of aliphatic polyols or their alkylene oxide adducts can be used. For example, diglycidyl ethers of alkylene glycols such as diglycidyl ether of ethylene glycol, diglycidyl ether of propylene glycol, and diglycidyl ether of 1,6-hexanediol, polyglycidyl ethers of polyols such as glycerol or its di- or triglycidyl ethers, diglycidyl ethers of polyethylene glycol or its alkylene oxide adducts, diglycidyl ethers of polyalkylene glycols such as diglycidyl ethers of polypropylene glycol or its alkylene oxide adducts, etc. Here, examples of the alkylene oxide include ethylene oxide and propylene oxide.

[0142] Among these epoxides, aromatic epoxides or alicyclic epoxides are preferred, and alicyclic epoxides are more preferred, from the viewpoint of curability.

[0143] As for the epoxy compound, one or more types can be appropriately selected and used.

[0144] As the oxetane compound, a compound having 1 to 4 oxetanyl groups in one molecule is preferred, and a compound having 2 to 4 oxetanyl groups in one molecule is more preferred.

[0145] Specific examples of the oxetane compound include 3-ethyl-3-[[(3-ethyloxetan-3-yl)methoxy]methyl]oxetane, 3-ethyl-3-hydroxymethyloxetane, 4,4'-bis[(3-ethyl-3-oxetan-3-yl)methoxymethyl]biphenyl, 3-(methyl)allyloxymethyl-3-ethyloxetane, (3-ethyl-3-oxetan-3-ylmethoxy)methylbenzene, (3-ethyl-3-oxetan-3-ylmethoxy)benzene, 4-fluoro-[1-(3-ethyl-3-oxetan-3-ylmethoxy)methyl]benzene, 4-methoxy-[1-(3-ethyl-3-oxetan-3-ylmethoxy)methyl]benzene, [1-(3-ethyl-3-oxetan-3-ylmethoxy)methyl]benzene, phenyl ether, isobutoxymethyl (3-ethyl-3-oxetanylmethyl) ether, isobornyloxyethyl (3-ethyl-3-oxetanylmethyl) ether, isobornyl (3-ethyl-3-oxetanylmethyl) ether, 2-ethylhexyl (3-ethyl-3-oxetanylmethyl) ether, ethyldiethylene glycol (3-ethyl-3-oxetanylmethyl) ether, dicyclopentadiene (3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyloxyethyl (3-ethyl-3-oxetanylmethyl) ether, dicyclopentyl (3-ethyl-3-oxetanylmethyl) ether, tetrahydrofurfuryl (3-ethyl-3-oxetanylmethyl) ether, tetrabromophenyl (3-ethyl-3-oxetanylmethyl) ether, 2-Tetrabromophenoxyethyl-(3-ethyl-3-oxetanylmethyl) ether, tribromophenyl-(3-ethyl-3-oxetanylmethyl) ether, 2-tribromophenoxyethyl-(3-ethyl-3-oxetanylmethyl) ether, butoxyethyl-(3-ethyl-3-oxetanylmethyl) ether, pentachlorophenyl-(3-ethyl-3-oxetanylmethyl) ether, pentabromophenyl-(3-ethyl-3-oxetanylmethyl) ether, bornyl-(3-ethyl-3-oxetanylmethyl) ether, 3,7-bis(3-oxetanyl)-5-oxanonane, 3,3'-[1,3-(2-methylene)-propylenediylbis(oxymethylene)]-bis(3-ethyloxetane), 1,4-bis[(3-ethyl-3 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, dicyclopentenyl bis(3-ethyl-3-oxetanylmethyl) ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, tricyclodecanediyl dimethylene-(3-ethyl-3-oxetanylmethyl) ether, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl) ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, pentaerythritol tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetra(3-ethyl-3-oxetanylmethyl) ether, polyethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol penta(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol tetra(3-ethyl-3-oxetanylmethyl) ether, caprolactone-modified dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl) ether, caprolactone-modified Dipentaerythritol penta(3-ethyl-3-oxetanyl methyl) ether, ditrimethylolpropane tetra(3-ethyl-3-oxetanyl methyl) ether, ethylene oxide modified bisphenol A-bis(3-ethyl-3-oxetanyl methyl) ether, propylene oxide modified bisphenol A-bis(3-ethyl-3-oxetanyl methyl) ether, ethylene oxide modified hydrogenated bisphenol A-bis(3-ethyl-3-oxetanyl methyl) ether, propylene oxide modified hydrogenated bisphenol A-bis(3-ethyl-3-oxetanyl methyl) ether, ethylene oxide modified bisphenol F-(3-ethyl-3-oxetanyl methyl) ether, etc.

[0146] As for the oxetane compound, one or two or more kinds can be appropriately selected and used.

[0147] As the vinyl ether compound, from the viewpoint of curability and adhesion, a di- or tri-vinyl ether compound is preferred, and a divinyl ether compound is more preferred.

[0148] Examples of the vinyl ether compound include di- or trivinyl ether compounds such as ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, propylene glycol divinyl ether, dipropylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, cyclohexanedimethanol divinyl ether, and trimethylolpropane trivinyl ether.

[0149] In addition, monovinyl ether compounds such as ethyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, octadecyl vinyl ether, cyclohexyl vinyl ether, hydroxybutyl vinyl ether, 2-ethylhexyl vinyl ether, cyclohexanedimethanol monovinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, isopropenyl ether-o-propylene carbonate, dodecyl vinyl ether, diethylene glycol monovinyl ether, and octadecyl vinyl ether can also be mentioned.

[0150] As for the vinyl ether compound, one or two or more kinds can be appropriately selected and used.

[0151] As the cationic polymerizable compound, it is more preferable to use an oxetane compound and an epoxy compound (particularly an alicyclic epoxide) in combination. The inventors of this application have determined that such a combination can improve the curability of the inkjet ink. Furthermore, compared to using an epoxy compound alone, the metallic gloss of the resulting image tends to be enhanced.

[0152] When an oxetane compound and an epoxy compound are used together, the ratio (mass %) of the epoxy compound, i.e., {amount of epoxy compound ÷ (amount of oxetane compound + amount of epoxy compound)} × 100, is preferably 15 to 85% by mass, and more preferably 20 to 80% by mass. By increasing the ratio of the epoxy compound to a certain extent, better curability is easily obtained. Furthermore, by not excessively increasing the ratio of the epoxy compound, storage stability tends to be further improved (thickness increase is easily suppressed).

[0153] When the inkjet ink of this embodiment contains a cationically polymerizable compound, the amount thereof is not particularly limited. When the total nonvolatile components (components other than the volatile organic solvent) in the ink are taken as 100% by mass, the amount thereof is generally 70 to 99.9% by mass, preferably 85 to 99.5% by mass, and more preferably 90 to 99% by mass.

[0154] Cationic polymerization initiator

[0155] As the cationic polymerization initiator, any substance can be used as long as it can generate cations upon external stimulation such as light irradiation and polymerize the above-mentioned cationically polymerizable compound. For example, onium salts can be used, and more specifically, known photocationic polymerization initiators such as sulfonium salt derivatives and iodonium salt derivatives can be used.

[0156] More specifically, cationic polymerization initiators include diazonium salts, iodonium salts, and sulfonium salts. These are composed of a cation portion that is an aromatic diazonium, an aromatic iodonium, or an aromatic sulfonium, and an anion portion that is BF4. - PF6 - 、SbF6 - 、[BX4] - (X is a phenyl group substituted with at least two fluorine or trifluoromethyl groups), (Rf) n PF 6-n (Rf is a fluorinated group such as a fluoroalkyl group, and n is an integer of 0=6) etc.

[0157] Specific examples of the compound include phenyldiazonium salts of boron tetrafluoride, diphenyliodonium salts of phosphorus hexafluoride, diphenyliodonium salts of antimony hexafluoride, tri-4-methylphenylsulfonium salts of arsenic hexafluoride, tri-4-methylphenylsulfonium salts of antimony tetrafluoride, diphenyliodonium salts of tetrakis(pentafluorophenyl)boron, a mixture of aluminum acetylacetonate and o-nitrobenzylsilyl ether, phenylthiopyridinium salts, and phosphorus hexafluoride allene-iron complexes.

[0158] Examples of commercially available cationic polymerization initiators include photocationic polymerization initiators such as CPI-100P, CPI-101A, and CPI-200K (manufactured by Sunapro), and WPI-113 and WPI-124 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).

[0159] The inkjet ink of the present embodiment may contain only one type of cationic polymerization initiator, or may contain two or more types of cationic polymerization initiators.

[0160] The amount of cationic polymerization initiator in the inkjet ink of this embodiment is not particularly limited. The amount is generally 0.5 to 15 parts by mass, preferably 1.0 to 10 parts by mass, more preferably 2 to 8 parts by mass, and particularly preferably 3 to 6 parts by mass, relative to 100 parts by mass of the cationically polymerizable compound. By appropriately adjusting the amount of cationic polymerization initiator, it is possible to achieve both higher levels of storage stability and curability.

[0161] Next, the radical polymerizable compound and the radical polymerization initiator in the above (ii) will be described.

[0162] Free radical polymerizable compounds

[0163] Examples of the radical polymerizable compound include compounds having one or two or more polymerizable carbon-carbon double bonds in one molecule (radical polymerizable monomers). The radical polymerizable compound is preferably a compound having one or two or more (meth)acryloyl groups in one molecule.

[0164] Examples of the monofunctional monomer (a compound having only one polymerizable carbon-carbon double bond in one molecule) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-stearyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dimethyl (meth)acrylamide, diethyl (meth)acrylamide, di-n-propyl (meth)acrylamide, and dibutyl (meth)acrylamide.

[0165] Examples of the polyfunctional monomer (a compound having two or more, preferably 2 to 6, polymerizable carbon-carbon double bonds in one molecule) include bifunctional monomers such as triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dihydroxymethyl-tricyclodecane di(meth)acrylate, PO adduct di(meth)acrylate of bisphenol A, hydroxypivalic acid neopentyl glycol di(meth)acrylate, and polytetramethylene glycol di(meth)acrylate.

[0166] Examples of the polyfunctional monomer include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, EO-modified pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerol propoxy tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, pentaerythritol ethoxy tetra(meth)acrylate, and caprolactam-modified dipentaerythritol hexa(meth)acrylate.

[0167] From a different viewpoint from the number of polymerizable functional groups, a monomer having a polar group (eg, a phosphoric acid group, a carboxyl group) can be used as the radical polymerizable monomer.

[0168] Examples of the monomer having a phosphoric acid group include 2-(meth)acryloyloxyethyl acid phosphate, di(2-methacryloyloxyethyl) acid phosphate, caprolactone-modified 2-acryloyloxyethyl acid phosphate, and diphenyl-2-acryloyloxyethyl phosphate.

[0169] Examples of the monomer having a carboxyl group include (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, citraconic acid, 2-(meth)acryloyloxymethylsuccinic acid, and 2-(meth)acryloyloxyethylsuccinic acid.

[0170] Inkjet inks may contain only one free radical polymerizable monomer or two or more. From the perspectives of appropriate polymerizability, crosslink density, and adhesion, for example, it is preferred to use a combination of monofunctional monomers and polyfunctional monomers. Furthermore, from the perspectives of adjusting adhesion and the dispersibility of the ink, it is preferred to use a combination of a monomer having a polar group and a monomer not having a polar group.

[0171] When the inkjet ink of this embodiment contains a radical polymerizable monomer, the amount thereof is not particularly limited. When the total nonvolatile component (components other than the volatile organic solvent) in the ink is taken as 100% by mass, the amount thereof is generally 85 to 99.5% by mass, preferably 90 to 99% by mass.

[0172] Free radical polymerization initiator

[0173] The radical polymerization initiator is not particularly limited as long as it can generate radicals upon external stimulation such as light irradiation to polymerize the above-mentioned radical polymerizable monomer.

[0174] Specific examples of free radical polymerization initiators include α-hydroxyketone photoinitiators, α-aminoketone photoinitiators, bisacylphosphine photoinitiators, monoacylphosphine oxides, bisacylphosphine oxides, for example, 2,4,6-trimethylbenzoylbiphenylphosphine oxide, ethyl-2,4,6-trimethylbenzoylphenylphosphinate, mono- and bis-acylphosphine photoinitiators, benzyl dimethyl ketal photoinitiators, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], and the like.

[0175] Commercially available radical polymerization initiators include photoradical polymerization initiators such as the IRGACURE (registered trademark) series sold by BASF Corp. Of course, other radical polymerization initiators may also be used.

[0176] The inkjet ink of the present embodiment may contain only one radical polymerization initiator, or may contain two or more radical polymerization initiators.

[0177] The amount of the radical polymerization initiator in the inkjet ink of the present embodiment is not particularly limited, but is generally 0.5 to 15 parts by mass, preferably 1.0 to 10 parts by mass, relative to 100 parts by mass of the radical polymerizable monomer.

[0178] (Other ingredients)

[0179] The inkjet ink of this embodiment may further include any other components in addition to the above-mentioned components. Examples of such optional components include dispersants, defoamers, leveling agents, polymerization inhibitors, waxes, antioxidants, non-reactive polymers, inorganic particulate fillers, silane coupling agents, light stabilizers, UV absorbers, antistatic agents, slip agents, storage stabilizers, and solvents (typically organic solvents). The inkjet ink of this embodiment may include one or more of these components.

[0180] From the viewpoint of improving adhesion, the inkjet ink of this embodiment preferably contains a silane coupling agent. In particular, when the inkjet ink of this embodiment is a cationic polymerization type, it is preferable to use a silane coupling agent.

[0181] Examples of silane coupling agents include aminosilane, epoxysilane, (meth)acrylic silane, mercaptosilane, vinylsilane, ureidosilane, and sulfide silane. Epoxysilane (a compound having an epoxy group and a hydrolyzable silyl group) is particularly preferred from the perspectives of improving adhesion and compatibility with the above-mentioned cationic polymerizable compounds.

[0182] As aminosilanes, for example, bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldiethoxysilane, or N-phenyl-γ-amino-propyltrimethoxysilane.

[0183] Examples of the epoxysilane include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and γ-glycidylpropyltrimethoxysilane.

[0184] Examples of the acrylic silane include γ-(methacryloxypropyl)trimethoxysilane, γ-(methacryloxypropyl)methyldimethoxysilane, and γ-(methacryloxypropyl)methyldiethoxysilane.

[0185] Examples of mercaptosilane include 3-mercaptopropyltrimethoxysilane and the like.

[0186] Examples of the vinylsilane include vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, and vinyltrimethoxysilane.

[0187] Examples of ureidosilane include 3-ureidopropyltriethoxysilane and the like.

[0188] Examples of the sulfide silane include bis(3-(triethoxysilyl)propyl)disulfide and bis(3-(triethoxysilyl)propyl)tetrasulfide.

[0189] When the inkjet ink of the present embodiment contains a silane coupling agent, it may contain only one type or two or more types.

[0190] When the inkjet ink of this embodiment contains a dispersant, the amount thereof is usually 0.1 to 30% by mass, preferably 1 to 20% by mass, based on 100% by mass of the total nonvolatile components (components other than the volatile organic solvent) in the ink.

[0191] The inkjet ink of this embodiment preferably contains a dispersant.

[0192] To further improve the dispersibility of flaky metal particles, surface modification of the flaky metal particles, as described above, is one method. However, the dispersibility of flaky metal particles can also be improved by using a dispersant in conjunction with or independently of surface modification. Dispersants include a variety of dispersants, including those containing acid groups, those containing amine structures, and those containing other polar groups. Both low-molecular-weight and high-molecular-weight dispersants are also available. In this embodiment, any dispersant can be used as long as it does not excessively impair the curability and storage stability of the inkjet ink.

[0193] According to the inventors of this application, it is preferred to use a dispersant containing an acid group as the dispersant. Although the details are unclear, it is believed that the acid group interacts well with the surface of the flaky metal particles. In addition, as another viewpoint, it is preferred to use a polymer-type dispersant as the dispersant.

[0194] As the dispersant, a commercially available product can be used, and examples of the commercially available dispersant include BYK's "DISPERBYK" series and "CERATIX" series, TEGO's "DISPERS" series, and Lubrizol's "Solsperse" series.

[0195] When the inkjet ink of the present embodiment contains a dispersant, it may contain only one type of dispersant or may contain two or more types of dispersants.

[0196] When the inkjet ink of this embodiment contains a dispersant, the amount thereof is usually 0.01 to 4 mass %, preferably 0.01 to 2 mass %, based on 100 mass % of the total nonvolatile components (components other than the volatile organic solvent) in the ink.

[0197] The inkjet ink of this embodiment preferably contains a storage stabilizer.

[0198] Examples of the storage stabilizer include amine compounds such as triethanolamine, triisopropanolamine, ethyl p-dimethylaminobenzoate, p-formyldimethylaniline, and p-methylthiodimethylaniline; thiol compounds such as 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 2-mercaptobenzimidazole, 2-mercapto-4(3H)-quinazoline, and β-mercaptonaphthalene, and their sulfides or disulfides; amino acid compounds such as N-phenylglycine; organometallic compounds such as tributyltin acetate; hydrogen donors; sulfur compounds such as trithiane; phosphorus compounds such as diethyl phosphite, and the like.

[0199] When using a storage stabilizer, only one type may be used, or two or more types may be used in combination.

[0200] When a storage stabilizer is used, the amount thereof is, for example, 0.03 to 0.15% by mass, and preferably 0.05 to 0.12% by mass, based on the total non-volatile content of the inkjet ink.

[0201] The inkjet ink of this embodiment may or may not contain a solvent, as long as it has a viscosity and fluidity sufficient to be ejected from an inkjet head. It should be noted that even if a solvent is not intentionally used, for example, when the flaky metal particles as a raw material are in the form of a dispersion, the inkjet ink may contain a solvent.

[0202] The inkjet ink of this embodiment generally does not contain a solvent, or even if it does, the amount of solvent is, for example, 50% by mass or less, preferably 25% by mass or less, and more preferably 15% by mass or less of the total ink. From another perspective, the inkjet ink of this embodiment may contain, for example, 5% by mass or more of a solvent based on the total ink due to the introduction of solvent from the inkjet ink raw materials (e.g., the dispersion of flaky metal particles).

[0203] The inkjet ink of the present embodiment preferably has almost no volatilization of the solvent or the like and no penetration of the ink into the substrate at the stage where the ink is fixed to the substrate.

[0204] Although it depends on the inkjet head used, the viscosity of the inkjet ink of this embodiment is preferably 2 to 50 mPa·s, more preferably 8 to 25 mPa·s, from the viewpoint of appropriate discharge properties.

[0205] (Method for producing inkjet ink)

[0206] The inkjet ink of this embodiment can be obtained by thoroughly mixing the above-mentioned components. For mixing, methods and apparatuses known in the field of inks can be appropriately used.

[0207] <Printed Material Manufacturing Method and Printed Material>

[0208] A printed article (a printed article comprising a cured product of the inkjet ink) can be produced by a series of steps including an image forming step of discharging the inkjet ink of this embodiment onto a substrate surface to form an image and a curing step of curing the discharged inkjet ink. The portion of the cured product of the inkjet ink in the printed article has a metallic luster.

[0209] The image forming process can be performed using a known inkjet device (inkjet printer). That is, using a device equipped with an inkjet head that can discharge inkjet ink into fine droplets, the inkjet ink droplets are discharged onto the substrate surface to form an image on the substrate surface.

[0210] As the inkjet head, a piezoelectric inkjet head is preferred from the viewpoint of suppressing deterioration of the ink. Examples of commercially available inkjet heads include the KM1024 series from Konica Minolta.

[0211] In the image forming process, the volume of the droplets discharged from the inkjet head is not particularly limited, but is typically about 2 to 50 pL.

[0212] The density of the droplets discharged from the inkjet head during the image forming process is not particularly limited and may be appropriately determined in consideration of the specifications of the inkjet device, the design of the final printed material, and the like.

[0213] The movement method of the inkjet head in the image forming step is not particularly limited, and any method commonly used in inkjet printing, such as a single-pass method, a multi-pass method, or a scanning method, can be employed.

[0214] The substrate (the substrate to which the inkjet ink is discharged) in the image forming process is not particularly limited. The material of the substrate can be, for example, paper, wood, metal, glass, resin, rubber, stone, concrete, etc. In addition, as long as the inkjet ink can adhere closely, the substrate is not limited.

[0215] The curing process is typically a photocuring process. That is, when the inkjet ink is photocurable, the inkjet ink discharged and landed on the substrate surface is irradiated with active energy rays, thereby curing the inkjet ink. As the active energy ray, ultraviolet rays can be preferably used. When ultraviolet rays are used as the active energy ray, a mercury lamp, a metal halide lamp, etc. can be used. In addition, the cumulative light intensity can be, for example, 100 to 10,000 mJ / cm 2 .

[0216] When the inkjet ink is thermosetting, the ink is cured by heating using any means such as hot air, an oven, or a hot plate.

[0217] In addition, when the curing step is a photocuring step, heating may be further performed after irradiation with active energy rays. This heating is performed to improve adhesion, etc. When this heating is performed, the conditions can be set to, for example, 40 to 200°C for 1 to 60 minutes.

[0218] The embodiments of the present invention have been described above, but these are merely examples of the present invention, and various configurations other than those described above can be employed. In addition, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are included in the present invention.

[0219] Example

[0220] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, the present invention is not limited to the Examples.

[0221] <Preparation of flaky metal particles (metallic pigments)>

[0222] The following dispersions of flaky metal particles (metallic pigments) were prepared. The concentration of each dispersion, the average major diameter of the flaky metal particles contained in each dispersion, and the like are shown in the table below.

[0223] Indium pigment dispersions 1 to 3: Indium pigment dispersions obtained from Oike Industry Co., Ltd.

[0224] Indium pigment dispersion 4: Indium pigment dispersion 2 was surface treated as follows

[0225] Chrome pigment dispersion: Chrome pigment dispersion obtained from Oike Industry Co., Ltd.

[0226] Aluminum pigment dispersion: Aluminum paste obtained from Toyo Aluminum Co., Ltd.

[0227] The surface treatment (surface) modification for obtaining the indium pigment dispersion 4 was performed as follows.

[0228] The following (i) to (iii) were mixed, and the mixture was heated and stirred at 70° C. for 1 hour. Thus, a metallic pigment (scaly metal particles) whose surface was modified with a group containing an isostearyl group was obtained.

[0229] (i) 2100 parts by mass of indium pigment dispersion (20 parts by mass in terms of solid content)

[0230] (ii) Isostearyl acrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., NK ester S-1800A) 0.36 parts by mass

[0231] (iii) 0.10 parts by mass of 3-aminopropyltrimethoxysilane (KBM-903, manufactured by Shin-Etsu Chemical Co., Ltd.)

[0232] Each flaky metal particle was photographed under magnification using a scanning electron microscope (field emission SEM "S-4800" manufactured by Hitachi High-Technologies Corporation). The major axis (maximum length of each particle) and thickness of 50 particles randomly selected from the image were measured. The average major axis and average thickness were then calculated.

[0233] In addition, light scattering measurement was performed on some of the flaky metal particles under the following conditions, and the harmonic average particle size (Z-average particle size) weighted by the scattered light intensity was calculated.

[0234] Measuring device: Zeta sizer Nano ZS (manufactured by Malvern)

[0235] Measurement temperature: 25°C

[0236] Sample cell: glass sample cell

[0237] Preparation of measurement samples: Indium pigment dispersions 1 to 4 were diluted 1000-fold with propylene glycol methyl ether to prepare measurement samples. Chromium pigment dispersions were diluted 1000-fold with butyl acetate to prepare measurement samples.

[0238] <Preparation of Raw Materials for Photocationic Curing Inkjet Ink (Other Than Flake Metal Particles)>

[0239] In order to prepare a photocationically curable inkjet ink, the following materials were prepared as raw materials other than the scaly metal particles.

[0240] [Table 1]

[0241] Table 1

[0242]

[0243] <Manufacturing of Photocationic Curing Inkjet Ink>

[0244] The components described in the table below were thoroughly mixed to produce a photocationically curable inkjet ink.

[0245] In the tables below, the amounts of flaky metal particles and initiator are reported as solids. In other words, the inkjet inks listed in the tables below contain, in addition to the ingredients explicitly listed, organic solvent entrained from the flaky metal particle dispersion and initiator solution.

[0246] <Evaluation of Photocationic Curing Inkjet Ink>

[0247] (Curing properties)

[0248] Follow the steps below to perform the evaluation.

[0249] (1) The inkjet ink was applied to a glass plate (size: 10 cm×10 cm×5 mm) using a 6-mil applicator to a thickness of 10 μm to form an uncured film on the glass plate.

[0250] (2) A high-pressure mercury lamp (manufactured by EYE GRAPHIC Co., Ltd., UB041-5A / B 60 Hz) was used at a cumulative light intensity of 500 mJ / cm 2 The uncured film is irradiated with ultraviolet rays under the conditions of . Thus, the uncured film is converted into a cured film.

[0251] (3) The cured state of the cured film was evaluated according to the following evaluation criteria.

[0252] 5 points: Fully cured, no stickiness.

[0253] 4 points: Although it feels sticky, it does not leave fingerprints when touched with fingers.

[0254] 3 points: It feels sticky and leaves fingerprints when touched.

[0255] 2 points: When the coating film is touched with a finger, the coating component adheres to the finger and increases in viscosity (curing) occurs.

[0256] 1 point: No curing at all.

[0257] (Viscosity)

[0258] The viscosity was measured at 100 rpm and 25° C. using an E-type viscometer (RE-85 viscometer manufactured by Toki Sangyo) in accordance with JIS K 7117-1.

[0259] <Evaluation of Printed Materials Using Photocationic Curing Inkjet Ink>

[0260] (For production of printed materials with metallic luster and total light transmittance (perspective evaluation))

[0261] As an inkjet printer, an inkjet printer (Stage JET manufactured by Tritec Co., Ltd.) equipped with a piezoelectric inkjet head (KM 1024iL manufactured by Konica Minolta, ink droplet volume 32 pL) was prepared.

[0262] Using this printer, inkjet ink was ejected onto a glass plate (10 cm x 10 cm x 2 mm) for printing (solid printing) at a head temperature of 45°C, a resolution of 720 dpi, and 8-way multiplexing. The ink was immediately cured by ultraviolet irradiation. The plate was then heated at 120°C for 3 minutes. This produced a test plate (evaluation print) for evaluating the appearance and durability of the printed material.

[0263] For the UV irradiation after solid printing, the device attached to the above-mentioned printer was used. About 1 second after the ink was discharged, the UV irradiation was carried out at a dose of 500 mJ / cm 2 It is carried out by irradiating ultraviolet rays under conditions of .

[0264] (Metallic gloss: 60° gloss value)

[0265] The metallic gloss was evaluated by the 60° gloss value. Specifically, the 60° gloss of the obtained printed material for evaluation was measured using a gloss meter "Micro-Gloss" manufactured by BYK-Gardner GmbH.

[0266] (Total light transmittance (perspective evaluation))

[0267] The haze was measured using a haze meter NDH4000 manufactured by Nippon Denshoku Industries, Ltd. in accordance with JIS K 7361-1.

[0268] (Satellite Drops Review)

[0269] As an inkjet printer, an inkjet printer (Tritec, Stage JET) equipped with a piezoelectric inkjet head (Konica Minolta, KM 1024iL, ink droplet volume 32 pL) was prepared. Using this printer, a straight line with a width of 2 mm was drawn under the following conditions. This produced a printed material for satellite droplet evaluation.

[0270] [condition]

[0271] Nozzle temperature: 45°C

[0272] Resolution: 720dpi

[0273] Printing speed: 740mm / sec

[0274] Nozzle gap: 2mm

[0275] 8-way split multiplexing

[0276] The area with a length of 1 mm within a straight line with a width of 2 mm drawn on the printed material for satellite droplet evaluation and its surroundings were observed using a microscope (see Figure 1 ). Then, the satellite droplets are scored based on the following criteria to evaluate the adhesion of the satellite droplets to the surrounding area of ​​the straight line.

[0277] ·Number evaluation

[0278] 5 points: Fewer than 10 satellite droplets were observed.

[0279] 4 points: The number of satellite droplets observed is 10 or more and less than 20

[0280] 3 points: The number of satellite droplets observed is 20 or more and less than 30

[0281] 2 points: The number of satellite droplets observed is 30 or more and less than 50

[0282] 1 point: The number of satellite droplets observed is 50 or more

[0283] ·Flyout distance evaluation: The distance from the drawn straight line to the satellite droplet that is farthest from the straight line

[0284] 5 points: less than 0.5mm

[0285] 4 points: 0.5mm or more and less than 1.0mm

[0286] 3 points: 1.0mm or more and less than 1.5mm

[0287] 2 points: 1.5 mm or more and less than 3.0 mm

[0288] 1 point: 3.0mm or more

[0289] The compositions of the inkjet inks and the evaluation results are summarized in the table below.

[0290] [Table 2]

[0291]

[0292] As shown in the table above, in each example, using an inkjet ink containing 2-10% by mass of flaky metal particles with an average major diameter of 400 nm or less can suppress the generation of satellite droplets while producing an image with a high metallic luster. This achieves both a high metallic luster in the printed image and the suppression of satellite droplet generation, two properties that have been difficult to achieve simultaneously.

[0293] On the other hand, in Comparative Examples 1-1 using scaly metal particles having an average major axis exceeding 400 nm, although an image having high metallic luster could be provided, the evaluation score of satellite droplets was low.

[0294] A more detailed analysis of the table above shows that when flaky metal particles with an average major diameter of 200 nm or less were used as flaky metal particles, the number of satellite droplets was rated at 5 points. On the other hand, when flaky metal particles with an average major diameter of 200 to 400 nm were used as flaky metal particles, the number of satellite droplets was rated at 3 or 4 points (Examples 1-3 and 1-5). This indicates that using flaky metal particles with an average major diameter of 200 nm or less can further reduce the problem of satellite droplets.

[0295] In addition, Examples 1-4 using the indium pigment dispersion 4 as the surface-modified particles exhibited particularly good metallic luster.

[0296] <Preparation of Raw Materials for Photo-Radical Curable Inkjet Ink (Other Than Scaly Metal Particles)>

[0297] In order to prepare a photo-radical curable inkjet ink, the following materials were prepared as raw materials other than the scaly metal particles.

[0298] [Table 3]

[0299] Table 3

[0300]

[0301] <Manufacturing of Photo-Radical Curable Inkjet Ink>

[0302] The components described in the table below were thoroughly mixed to produce a photo-radical curable inkjet ink.

[0303] In the tables described below, the flaky metal particles are the same as those used in the above-mentioned photocationically curable inkjet ink.

[0304] <Evaluation of Photo-Radical Curable Inkjet Ink>

[0305] (Curing properties)

[0306] The five-stage evaluation was performed in the same procedure as for the photocationic curing inkjet ink.

[0307] (Viscosity)

[0308] The measurement was performed in the same manner as for the photocationically curable inkjet ink.

[0309] <Evaluation of Printed Materials Using Photo-Radical Curable Inkjet Ink>

[0310] (Production of evaluation printed materials, metallic gloss: 60° gloss value, total light transmittance (perspective evaluation), satellite droplet evaluation)

[0311] Preparation of printed materials for evaluation, score evaluation, etc. were performed in the same manner as in the case of the photocationically curable inkjet ink.

[0312] The composition, evaluation results, etc. of the photoradical curable inkjet ink are summarized in the table below.

[0313] [Table 4]

[0314]

[0315] As can be seen from the above table, not only in the photocationic curing type but also in the photoradical curing type, by preparing an inkjet ink containing 2 to 10% by mass of flaky metal particles with an average major diameter of 400 nm or less, the generation of satellite droplets can be suppressed and an image with high metallic gloss can be provided.

[0316] This application claims the benefit of priority based on Japanese patent application No. 2020-150318, filed on September 8, 2020, the disclosure of which is incorporated herein in its entirety.

Claims

1. An inkjet ink comprising flaky metal particles, The average major diameter of the flaky metal particles is 400 nm or less. The flaky metal particles are not surface-modified, or are surface-modified with an alkyl group having 4 or more carbon atoms, The inkjet ink contains 2 to 10% by mass of the flaky metal particles. The inkjet ink contains no dispersant or contains a dispersant containing an acid group.

2. The inkjet ink according to claim 1, wherein The average major diameter of the flaky metal particles is 50 to 200 nm.

3. The inkjet ink according to claim 1 or 2, wherein: The flaky metal particles include indium and / or chromium.

4. The inkjet ink according to claim 1 or 2, further comprising a radical polymerizable compound and a radical polymerization initiator.

5. The inkjet ink according to claim 4, wherein The radical polymerizable compound includes a compound having a (meth)acryloyl group.

6. The inkjet ink according to claim 1 or 2, further comprising a cationically polymerizable compound and a cationic polymerization initiator.

7. The inkjet ink according to claim 6, wherein The cationically polymerizable compound includes a compound having an epoxy group and / or an oxetanyl group.

8. The inkjet ink according to claim 1 or 2, which is photocurable.

9. A method for producing a printed matter, comprising: An image forming step of discharging the inkjet ink according to any one of claims 1 to 8 onto a substrate surface to form an image; and A curing step of curing the discharged inkjet ink. 10 . A printed matter comprising a cured product of the inkjet ink according to claim 1 .