Aluminum alloy 3D printing material, aluminum alloy 3D printing parts and preparation method

By using a combination of aluminum alloy powder, thermoplastic materials and sintering aids, using a hot extruder to shape and sinter in a vacuum sintering furnace, the problems of high cost and low safety of aluminum alloy 3D printing technology are solved, and high strength is achieved , low-cost and high-safety production of aluminum alloy 3D printed parts.

CN116083760BActive Publication Date: 2024-10-18CHINA FAW CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211416786.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-10-18
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

Existing aluminum alloy 3D printing technology is expensive and has low safety, mainly due to high equipment costs and powder materials that are harmful to the operator's health and are flammable and explosive.

Method used

A combination of aluminum alloy powder, thermoplastic materials, sintering aids and paraffin is used, formed through a hot extruder and sintered in a vacuum sintering furnace to form dense aluminum alloy parts, reducing equipment costs and improving safety.

Benefits of technology

It has realized the production of aluminum alloy 3D printed parts with low cost and high safety, with a tensile strength of 320MPa, a yield strength of 260MPa, an elongation of 12%, and reduced material manufacturing costs and finished product costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

Aluminum alloy 3D printing materials, aluminum alloy 3D printing parts and preparation methods, which relate to the technical field of 3D printing materials, solve the problems of high cost and low safety. The materials include the following components in volume percentage: aluminum alloy powder: 57% to 65%, thermoplastic material: 15% to 20%, sintering aid: 3% to 5%, paraffin wax 10% to 25%; aluminum alloy powder includes the following components in mass percentage: Si: 5% to 15%, Mn: 0.1% to 2%, Mg: 0.1% to 1%, Sr: 0.01% to 0.5%, Sn: 0.1% to 0.5%, other impurities ≤ 1%, and the balance is Al; thermoplastic material includes the following components in percentage: polyoxymethylene: 47% to 65%, polyetherimide: 8% to 12%, polystyrene: 13% to 16%, polyphenylene sulfide: 2% to 5%, palm oil wax: 2% to 30%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing materials, and in particular to an aluminum alloy 3D printing material, an aluminum alloy 3D printing part, and a preparation method thereof. Background Art

[0002] One of the most important development directions in the automotive industry is to design traditional fuel vehicles and new energy vehicles with lightweight design. Under the premise of ensuring the strength and safety performance of the vehicle, the curb weight of the vehicle is reduced as much as possible, thereby improving the vehicle's power, reducing fuel consumption, and reducing exhaust pollution. There are two ways to achieve lightweighting of vehicles. One is to use lightweight materials such as titanium alloys, aluminum alloys, magnesium alloys or carbon fiber composite materials to achieve the purpose of weight reduction; the second is to reduce weight through structural designs such as integration, integration, thin-walling, and hollowing.

[0003] For automotive products, based on comprehensive considerations of performance, cost, and technological maturity, among many lightweight materials, aluminum alloy materials are undoubtedly the first choice for lightweighting automobiles. Traditional aluminum alloy material forming methods mainly use casting or stamping, which require mold forming, and are limited by the mold structure and cannot maximize the space for lightweight structural design of parts. 3D printing uses a layer-by-layer stacking method according to the digital model to construct objects, which is not limited by the mold and brings more possibilities for lightweight structural design. It can realize hollow sandwich / thin-wall reinforced structures, lattice structures, integrated structures, special-shaped topological optimization structures, etc. that cannot be achieved by traditional processes. Therefore, the combination of 3D printing technology and aluminum alloy materials can overcome the shortcomings of traditional aluminum alloy forming and provide automotive designers with greater design freedom oriented towards product functions, thereby maximizing lightweighting.

[0004] The most successful aluminum alloy 3D printing technology in the automotive industry is powder bed melting technology. For example, Porsche 3D printed an aluminum alloy piston for the 911 flagship model GT2 RS, and designed a complete closed cooling duct on the top of the piston, which reduced the weight of the piston by 10% compared with the original; the BMW i8 Roadster uses 3D printed aluminum alloy convertible roof brackets, which reduced the weight of the part by 44% and improved the rigidity. Powder bed melting technology uses laser or electron beam as a heat source (SLM process uses laser, EBM process uses electron beam), melts the powder particles together point by point, and then metallurgically welds them with the base metal after heat dissipation and solidification, and then accumulates layer by layer to form a three-dimensional entity.

[0005] The performance of parts printed by this technology is comparable to that of parts processed by traditional processes. However, since this technology requires the use of devices such as lasers or electron beams to emit heat sources, the equipment cost is high. The equipment depreciation cost is allocated to each 3D printed part, resulting in expensive parts, which restricts its application. The aluminum alloy raw materials required for powder bed melting are all in powder form. Powder materials are not only harmful to the health of operators, but also easy to burn and explode under fire, static electricity, and friction and collision when reaching a certain concentration, posing a safety hazard. Summary of the invention

[0006] In order to solve the problems of high cost and low safety of the prior art, the present invention proposes an aluminum alloy 3D printing material, an aluminum alloy 3D printing part and a preparation method.

[0007] The technical solution of the present invention is as follows:

[0008] An aluminum alloy 3D printing material, comprising the following components in percentage by volume:

[0009] Aluminum alloy powder: 57%~65%, thermoplastic material: 15%~20%, sintering aid: 3%~5%, paraffin 10%~25%;

[0010] The aluminum alloy powder includes the following components in percentage by mass:

[0011] Si: 5%~15%, Mn: 0.1%~2%, Mg: 0.1%~1%, Sr: 0.01%~0.5%, Sn: 0.1%~0.5%, other impurities ≤1%, the balance is Al;

[0012] The aluminum alloy powder has a D50 particle size of 8 μm to 14 μm, a bulk density of 40% to 50%, and a tap density of 60% to 80%;

[0013] The thermoplastic material comprises the following components in percentage: polyoxymethylene: 47%-65%, polyetherimide: 8%-12%, polystyrene: 13%-16%, polyphenylene sulfide: 2%-5%, and palm oil wax: 2%-30%.

[0014] Preferably, the sintering aid is a mixture of any two or more of CaF2, SiO2 and MgO2.

[0015] A method for preparing the aluminum alloy 3D printing material as described above, characterized in that the method comprises the following steps:

[0016] S1. Add Al, Si, Mg, Mn, Sn and Sr powders into a mixer according to the component ratio and mix them evenly to obtain aluminum alloy powder;

[0017] S2, adding the thermoplastic material into a mixer according to the composition ratio, then adding paraffin wax, heating and mixing at a speed of 15 rpm to 20 rpm at 100° C. to 140° C. until the mixture is molten;

[0018] S3, mixing the aluminum alloy powder and the sintering aid, preheating them together to 90°C to 110°C, and then adding them to the molten mixture obtained in step S2, and continuing to heat and mix at 100°C to 140°C at a speed of 30rpm to 40rpm for 40min to 60min, while maintaining a vacuum state in the mixer;

[0019] S4. Add the mixture obtained in step S3 into a twin-screw extruder, and extrude the filament through a die to obtain an aluminum alloy 3D printing material.

[0020] Preferably, the feeding temperature of the twin-screw extruder in step S4 is 50°C to 90°C, the melting section temperature is 150°C to 180°C, the homogenizing section temperature is 140°C to 185°C, and the head and die section temperature is 180°C to 200°C.

[0021] A method for preparing an aluminum alloy 3D printed part, using the aluminum alloy 3D printed material as a raw material, the method comprises the following steps:

[0022] T1. Place the aluminum alloy 3D printing material on the hot extruder, heat and melt it through the nozzle, and extrude it onto the hot bed according to the cross-sectional contour of the 3D printed digital model. The material solidifies and condenses with the surrounding materials to complete the printing of one layer of contour. The next layer is printed in the same way, and so on, until the green body is obtained;

[0023] T2, soaking the green body in an organic solvent, heating and degreasing, so that the degreasing constant K = m1 / (m1-m2) × 100% satisfies K ≥ 4.2%, and then drying in a drying oven to obtain a brown mold; wherein m1 represents the mass of the green body, and m2 represents the mass of the brown mold;

[0024] T3. Place the brown mold that meets the conditions in a vacuum sintering furnace for sintering. Inert protective gas is introduced into the furnace to obtain aluminum alloy 3D printed parts.

[0025] Preferably, the nozzle temperature of the hot extruder in step T1 is 200° C. to 280° C., the hot bed temperature is 100° C. to 140° C., and the thickness of the printed single layer is 0.03 mm to 0.15 mm.

[0026] Preferably, the organic solvent in step T2 is trichloroethane solvent, high-purity tetrachloroethylene or trans-1,2-dichloroethylene.

[0027] Preferably, in step T2, the heating temperature is 60° C. to 90° C., the heating time is 12 h to 36 h, the drying temperature is 40° C. to 50° C., and the drying time is 8 h to 12 h.

[0028] Preferably, the specific process of sintering in step T3 is: first, the temperature is increased to 250°C to 320°C at a heating rate of 3°C / min to 6°C / min, and kept warm for 2h to 4h; then, the temperature is increased to 450°C to 660°C at a heating rate of 2°C / min to 5°C / min, and kept warm for 4h to 8h; then, the temperature is cooled with the furnace at a cooling rate of 8°C / min to 12°C / min; when the temperature in the furnace drops to room temperature, it is reheated to 150°C to 200°C at a heating rate of 3°C / min to 5°C / min, and kept warm for 3h to 5h; and the temperature is cooled with the furnace at a cooling rate of 5°C / min to 8°C / min.

[0029] Preferably, the inert protective gas in T3 is one or more mixed gases selected from argon, nitrogen and argon-hydrogen mixed gas, and the ratio of the argon-hydrogen mixed gas is argon:hydrogen=96%:4%.

[0030] Compared with the prior art, the present invention solves the problem of high cost and low safety of the existing aluminum alloy 3D printing technology, and the specific beneficial effects are:

[0031] 1. The present invention mixes aluminum alloy material and thermoplastic material to make wire, then forms the wire through a hot extruder, and then uses an organic solvent to heat and degrease to remove the thermoplastic material. Finally, through sintering, the aluminum alloy powders are allowed to flow, diffuse, and dissolve with each other, and metallurgical bonding is formed between the powders, thereby obtaining dense aluminum alloy parts; compared with laser / electron beam 3D printing equipment, the hot extruder used in the present invention has a lower cost. In addition, the raw materials of the present invention do not need to strictly restrict the powder particle size, powder shape, etc., thereby reducing the material manufacturing cost and the yield rate. The cost of 3D printed parts in the present invention can be reduced by 40% compared with the cost of 3D printed parts prepared by a powder bed.

[0032] 2. The raw material used in the present invention is in the form of wire, there is no dust in the 3D printing process, there is no special requirement for the operating environment, the operation is simple and the safety is high.

[0033] 3. The tensile strength of the parts provided by the present invention can reach 320MPa, the yield strength can reach 260MPa, and the elongation can reach 12%; the strength is the same as that of the prior art. DETAILED DESCRIPTION

[0034] In order to make the technical solution of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. It should be noted that the following embodiments are only used to better understand the technical solution of the present invention and should not be understood as limiting the present invention.

[0035] Example 1.

[0036] This embodiment provides an aluminum alloy 3D printing material, a preparation method, and a parts preparation method. The aluminum alloy 3D printing material includes the following components in percentage by volume:

[0037] Aluminum alloy powder 57%; thermoplastic material 17%; sintering aid 3%; paraffin 23%.

[0038] Wherein, the specific composition of the aluminum alloy powder is shown in Table 1 in terms of mass percentage of the aluminum alloy powder;

[0039] Table 1

[0040] Components Si Mn Mg Sr Sn Al Mass percentage / % 9.62 0.47 0.65 0.12 0.34 margin

[0041] The thermoplastic material is expressed in volume percentage, and the specific composition of the thermoplastic material is shown in Table 2;

[0042] Table 2

[0043] Components Polyoxymethylene Polyetherimide Polystyrene Polyphenylene sulfide Palm oil wax Volume percentage / % 49 12 15 3 21

[0044] The D50 particle size of aluminum alloy powder is 10um, the bulk density is 43%; the tap density is 65%;

[0045] The sintering aids are CaF2 and SiO2, with the volume ratio of CaF2:SiO2 being 40%:60%;

[0046] The preparation method of the above 3D printing material is as follows:

[0047] S1: According to the aluminum alloy composition in Table 1, the powders of Al, Si, Mg, Mn, Sn and Sr elements are mixed evenly in a mixer, and Si, Mg, Mn, Sn and Sr elements are added in the form of pre-alloyed powder and master alloy powder;

[0048] S2: Add the thermoplastic material into a mixer according to the composition ratio, add paraffin wax at the same time, heat and mix until molten, the mixer speed is 15 rpm, and the mixing temperature is 110°C;

[0049] S3: Mix the mixed aluminum alloy powder and sintering aid, preheat them together to 95°C, and then add them to the mixture obtained in step S2 to continue heating and mixing. The mixer is kept in a vacuum state, the mixer speed is 40 rpm, and the temperature is 110°C; mix for 60 minutes;

[0050] S4: adding the mixture obtained in step S3 to a twin-screw extruder to extrude a filament through a die, and then collecting the filament into a coil by a disc device to obtain the low-cost, high-safety 3D printing material, wherein the temperature of the feeding section of the twin-screw extruder is 50°C, the temperature of the melting section is 160°C, the temperature of the homogenizing section is 150°C, the temperature of the die section is 185°C, the temperature of the die section is 200°C, and the filament diameter is 0.5 mm.

[0051] The preparation method of the 3D printed parts is as follows:

[0052] T1: Place the rolled 3D printing filament prepared by the preparation method on a hot extruder, heat and melt the material through the nozzle of the hot extruder, and extrude it onto the hot bed according to the cross-sectional profile of the 3D printed digital model. The material solidifies and condenses with the surrounding materials. After one layer of contour printing is completed, the next layer is printed in the same way, and so on, until a green body is obtained; wherein, the temperature of the 3D printer nozzle is 230°C, the temperature of the hot bed is 110°C, and the thickness of each isolation layer is 0.050mm;

[0053] T2: soaking the green body obtained in step S1 in trichloroethane solvent for 18 hours at 75°C for degreasing, and then drying at 47°C for 9 hours to obtain a brown mold;

[0054] T3: The debinding constant is calculated to be 4.31%. The brown mold obtained in step S2 is placed in a vacuum sintering furnace, and the temperature is increased from room temperature to 270°C at a heating rate of 4°C / min, and kept at this temperature for 4 hours. The temperature is then increased to 560°C at a heating rate of 3°C / min, and kept at this temperature for 6 hours. The furnace is cooled at a cooling rate of 10°C / min. When the temperature in the furnace drops to room temperature, the temperature is increased to 170°C at a heating rate of 3°C / min again, and kept at this temperature for 3 hours. The furnace is cooled at a cooling rate of 6°C / min to obtain a 3D printed part. During the sintering process, high-purity argon is introduced into the furnace as a protective gas.

[0055] Example 2

[0056] This embodiment provides an aluminum alloy 3D printing material, a preparation method, and a parts preparation method. The aluminum alloy 3D printing material includes the following components in percentage by volume:

[0057] Aluminum alloy powder 61%; thermoplastic material 20%; sintering aid 4%; paraffin 15%.

[0058] Wherein, the specific composition of the aluminum alloy powder is shown in Table 3 in terms of mass percentage of the aluminum alloy powder;

[0059] Table 3

[0060] Components Polyoxymethylene Polyetherimide Polystyrene Polyphenylene sulfide Palm oil wax Volume percentage / % 55 10 13 5 17

[0061] The thermoplastic material is expressed in volume percentage, and the specific composition of the thermoplastic material is shown in Table 4;

[0062] Table 4

[0063] element Si Mn Mg Sr Sn Al Mass percentage / % 6.73 1.23 0.87 0.05 0.25 margin

[0064] The D50 particle size of aluminum alloy powder is 12um, the bulk density is 50%; the tap density is 76%;

[0065] The sintering aids are CaF2 and MgO2, with the volume ratio of CaF2:MgO2 being 50%:50%;

[0066] The preparation method of the above-mentioned low-cost and high-safety 3D printing material is as follows:

[0067] S1: According to the aluminum alloy composition in Table 1, the powders of Al, Si, Mg, Mn, Sn and Sr elements are mixed evenly in a mixer, and Si, Mg, Mn, Sn and Sr elements are added in the form of pre-alloyed powder and master alloy powder;

[0068] S2: Add the thermoplastic material into a mixer according to the composition ratio, add paraffin wax at the same time, heat and mix until molten, the mixer speed is 20 rpm, and the mixing temperature is 130°C;

[0069] S3: Mix the mixed aluminum alloy powder and sintering aid, preheat them together to 100°C, and then add them to the mixture obtained in step S2 to continue heating and mixing. The mixer is kept in a vacuum state, the mixer speed is 30 rpm, and the temperature is 130°C; mix for 50 minutes;

[0070] S4: adding the mixture obtained in step S3 to a twin-screw extruder to extrude a filament through a die, and then collecting the filament into a coil by a disc device to obtain the low-cost, high-safety 3D printing material, wherein the temperature of the feeding section of the twin-screw extruder is 70°C, the temperature of the melting section is 180°C, the temperature of the homogenizing section is 165°C, the temperature of the die section is 190°C, the temperature of the die section is 200°C, and the filament diameter is 0.8 mm.

[0071] The preparation method of the 3D printed parts is as follows:

[0072] T1: Place the rolled 3D printing filament prepared by the preparation method on a hot extruder, heat and melt the material through the nozzle of the hot extruder, and extrude it onto the hot bed according to the cross-sectional contour of the 3D printed digital model. The material solidifies and condenses with the surrounding materials. After one layer of contour printing is completed, the next layer is printed in the same way, and so on, until a green body is obtained; wherein, the temperature of the 3D printer nozzle is 250℃, the temperature of the hot bed is 120℃, and the thickness of each isolation layer is 0.10mm;

[0073] T2: soaking the green body obtained in step S1 in trichloroethane solvent for 16 hours at 80°C for degreasing, and then drying at 50°C for 8 hours to obtain a brown mold;

[0074] T3: The debinding constant is calculated to be 4.27%. The brown mold obtained in step S2 is placed in a vacuum sintering furnace, and the temperature is increased from room temperature to 300°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours. Then, the temperature is increased to 600°C at a heating rate of 5°C / min, and kept at this temperature for 5 hours. The furnace is cooled at a cooling rate of 9°C / min. When the temperature in the furnace drops to room temperature, the temperature is increased to 150°C at a heating rate of 4°C / min again, and kept at this temperature for 5 hours. The furnace is cooled at a cooling rate of 7°C / min to obtain a 3D printed part. During the sintering process, high-purity nitrogen is introduced into the furnace as a protective gas.

[0075] Example 3.

[0076] This embodiment provides an aluminum alloy 3D printing material, a preparation method, and a parts preparation method. The aluminum alloy 3D printing material includes the following components in percentage by volume:

[0077] Aluminum alloy powder 65%; thermoplastic material 18%; sintering aid 5%; paraffin 12%.

[0078] Wherein, the specific composition of the aluminum alloy powder is shown in Table 5 in terms of mass percentage of the aluminum alloy powder;

[0079] Table 5

[0080] Components Polyoxymethylene Polyetherimide Polystyrene Polyphenylene sulfide Palm oil wax Volume percentage / % 64 8 14 4 10

[0081] The thermoplastic material is expressed in volume percentage, and the specific composition of the thermoplastic material is shown in Table 6;

[0082] Table 6

[0083] element Si Mn Mg Sr Sn Al Mass percentage / % 11.7 0.58 0.37 0.14 0.28 margin

[0084] The D50 particle size of aluminum alloy powder is 14um, the bulk density is 45%; the tap density is 68%;

[0085] The sintering aids are CaF2, SiO2, and MgO2, wherein the volume ratio of CaF2:SiO2:MgO2 is 40%:40%:20%;

[0086] The preparation method of the above 3D printing material is as follows:

[0087] S1: According to the aluminum alloy composition in Table 1, the powders of Al, Si, Mg, Mn, Sn and Sr elements are mixed evenly in a mixer, and Si, Mg, Mn, Sn and Sr elements are added in the form of pre-alloyed powder and master alloy powder;

[0088] S2: Add the thermoplastic material into a mixer according to the composition ratio, add paraffin wax at the same time, heat and mix until molten, the mixer speed is 18 rpm, and the mixing temperature is 140°C;

[0089] S3: Mix the mixed aluminum alloy powder and sintering aid, preheat them together to 110°C, and then add them to the mixture obtained in step S2 to continue heating and mixing. The mixer is kept in a vacuum state, the mixer speed is 35 rpm, and the temperature is 140°C; mix for 40 minutes;

[0090] S4: adding the mixture obtained in step S3 to a twin-screw extruder to extrude a filament through a die, and then collecting the filament into a coil by a disc device to obtain the low-cost, high-safety 3D printing material, wherein the temperature of the feeding section of the twin-screw extruder is 80°C, the temperature of the melting section is 175°C, the temperature of the homogenizing section is 180°C, the temperature of the die head is 195°C, the temperature of the die section is 195°C, and the filament diameter is 1.0 mm.

[0091] The preparation method of the 3D printed parts is as follows:

[0092] T1: Place the rolled 3D printing filament prepared by the preparation method on a hot extruder, heat and melt the material through the nozzle of the hot extruder, and extrude it onto the hot bed according to the cross-sectional profile of the 3D printed digital model. The material solidifies and condenses with the surrounding materials. After one layer of contour printing is completed, the next layer is printed in the same way, and so on, until a green body is obtained; wherein, the temperature of the 3D printer nozzle is 270°C, the temperature of the hot bed is 120°C, and the thickness of each isolation layer is 0.125mm;

[0093] T2: soaking the green body obtained in step S1 in trichloroethane solvent for 30 hours at 60°C for degreasing, and then drying at 40°C for 12 hours to obtain a brown mold;

[0094] T3: The debinding constant is calculated to be 4.35%. The brown mold obtained in step S2 is placed in a vacuum sintering furnace, and the temperature is increased from room temperature to 250°C at a heating rate of 3°C / min, and kept at this temperature for 3 hours. Then, the temperature is increased to 640°C at a heating rate of 4°C / min, and kept at this temperature for 4 hours. The temperature is cooled with the furnace at a cooling rate of 12°C / min. When the temperature in the furnace drops to room temperature, the temperature is increased to 200°C at a heating rate of 5°C / min again, kept at this temperature for 4 hours, and cooled with the furnace at a cooling rate of 8°C / min to obtain a 3D printed part. During the sintering process, an argon-hydrogen mixed gas is introduced into the furnace as a protective gas, wherein argon:hydrogen = 96%:4%.

[0095] Example 4.

[0096] The parts prepared in the above three embodiments were tested according to GB / T228.1-2021 standard. The performance indicators are shown in Table 7. It can be seen that the tensile strength exceeds 320 MPa, the yield strength exceeds 260 MPa, and the elongation exceeds 12%;

[0097] Table 7

[0098]

[0099] The cost of the parts prepared by the above embodiment is compared with the cost of the same parts prepared by laser 3D printing, as shown in Table 8.

[0100] Table 8

[0101]

Claims

1. A method for preparing aluminum alloy 3D printed parts, It is characterized in that The aluminum alloy 3D printing material is used as a raw material, and the aluminum alloy 3D printing material includes the following components in volume percentage: Aluminum alloy powder: 57%~65%, thermoplastic material: 15%~20%, sintering aid: 3%~5%, paraffin 10%~25%; The aluminum alloy powder includes the following components in percentage by mass: Si: 5%~15%, Mn: 0.1%~2%, Mg: 0.1%~1%, Sr: 0.01%~0.5%, Sn: 0.1%~0.5%, other impurities ≤1%, the balance is Al; The aluminum alloy powder has a D50 particle size of 8 μm to 14 μm, a bulk density of 40% to 50%, and a tap density of 60% to 80%; The thermoplastic material comprises the following components in percentage: polyoxymethylene: 47% to 65%, polyetherimide: 8% to 12%, polystyrene: 13% to 16%, polyphenylene sulfide: 2% to 5%, and palm oil wax: 2% to 30%; The sintering aid is CaF 2 、SiO 2 and MgO 2 A mixture of any two or more of the following; The method for preparing the aluminum alloy 3D printed parts comprises the following steps: T1. Place the aluminum alloy 3D printing material on the hot extruder, heat and melt it through the nozzle, and extrude it onto the hot bed according to the cross-sectional contour of the 3D printed digital model. The material solidifies and condenses with the surrounding materials to complete the printing of one layer of contour. The next layer is printed in the same way, and so on, until the green body is obtained; T2, immerse the green body in an organic solvent and heat to degrease, so that the degreasing constant K = (m 1 -m 2 ) / m 1 ×100% satisfies K≥4.2%, and then placed in a drying oven to dry to obtain a brown mold; wherein, m 1 Represents the green mass, m 2 Represents the quality of brown mold; T3. Place the brown mold that meets the conditions in a vacuum sintering furnace for sintering, introduce inert protective gas into the furnace, and obtain aluminum alloy 3D printed parts; The specific process of sintering in step T3 is: first, the temperature is increased to 250°C to 320°C at a heating rate of 3°C / min to 6°C / min, and kept warm for 2h to 4h; then, the temperature is increased to 450°C to 660°C at a heating rate of 2°C / min to 5°C / min, and kept warm for 4h to 8h; then, the temperature is cooled with the furnace at a cooling rate of 8°C / min to 12°C / min; when the temperature in the furnace drops to room temperature, it is reheated to 150°C to 200°C at a heating rate of 3°C / min to 5°C / min, and kept warm for 3h to 5h; and the temperature is cooled with the furnace at a cooling rate of 5°C / min to 8°C / min.

2. A method for preparing an aluminum alloy 3D printed part as claimed in claim 1, It is characterized in that The aluminum alloy 3D printing material is prepared by the following steps: S1. Add Al, Si, Mg, Mn, Sn and Sr powders into a mixer according to the component ratio and mix them evenly to obtain aluminum alloy powder; S2, adding the thermoplastic material into a mixer according to the composition ratio, then adding paraffin wax, heating and mixing at a speed of 15 rpm to 20 rpm at 100° C. to 140° C. until the mixture is molten; S3, mixing the aluminum alloy powder and the sintering aid, preheating them together to 90°C to 110°C, and then adding them to the molten mixture obtained in step S2, and continuing to heat and mix at 100°C to 140°C at a speed of 30rpm to 40rpm for 40min to 60min, while maintaining a vacuum state in the mixer; S4. Add the mixture obtained in step S3 into a twin-screw extruder, and extrude the filament through a die to obtain an aluminum alloy 3D printing material.

3. The method for preparing aluminum alloy 3D printed parts according to claim 2, It is characterized in that The feeding temperature of the twin-screw extruder in step S4 is 50°C to 90°C, the melting section temperature is 150°C to 180°C, the homogenizing section temperature is 140°C to 185°C, and the head and die section temperature is 180°C to 200°C.

4. The method for preparing aluminum alloy 3D printed parts according to claim 1, It is characterized in that The nozzle temperature of the hot extruder in step T1 is 200° C. to 280° C., the hot bed temperature is 100° C. to 140° C., and the thickness of the printed single layer is 0.03 mm to 0.15 mm.

5. The method for preparing aluminum alloy 3D printed parts according to claim 1, It is characterized in that The organic solvent in step T2 is trichloroethane solvent, high-purity tetrachloroethylene or trans-1,2-dichloroethylene.

6. The method for preparing aluminum alloy 3D printed parts according to claim 1, It is characterized in that In step T2, the heating temperature is 60° C. to 90° C., the heating time is 12 h to 36 h, the drying temperature is 40° C. to 50° C., and the drying time is 8 h to 12 h.

7. The method for preparing aluminum alloy 3D printed parts according to claim 1, It is characterized in that The inert protective gas in T3 is one or more mixed gases selected from argon, nitrogen and argon-hydrogen mixed gas, and the ratio of the argon-hydrogen mixed gas is argon:hydrogen=96%:4%.

Citation Information

Patent Citations

  • Die casting aluminum alloy and preparation method thereof

    CN104451278A

  • Manufacturing method for automobile metal support parts

    CN110405213A

  • Die-casting aluminum alloy and automotive component

    CN110541094A

  • Polymer composite stainless steel 3D printing material, preparation method and preparation method of part

    CN111940739A

  • Laminate-molding metal powder, laminate-molded article manufacturing method, and laminate-molded article

    WO2017203717A1