Nanosheets and their formation methods
By using alternating stacked sacrificial oxide and nitride layers in nanosheet fabrication to form multiple trenches and through-grooves, the problems of germanium diffusion and interface defects are solved, thereby improving the applicability and device quality of nanosheets.
Patent Information
- Application Number
- CN202211685832.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-27
AI Technical Summary
In existing nanosheet manufacturing technologies, germanium diffusion from the silicon-germanium layer into the silicon layer leads to compressive stress and silicon-germanium interface defects, affecting the yield and quality of semiconductor devices.
Multiple trenches and through-grooves are formed by alternating stacked multilayer sacrificial oxide layers and multilayer sacrificial nitride layers. The sacrificial nitride layer is removed and an epitaxial growth structure is formed in the exposed space. This avoids germanium diffusion and interface defects, forming a stacked nanosheet layer in which the epitaxial growth structure and the sacrificial oxide layer are stacked alternately.
It effectively solves the problems of compressive stress in the channel of semiconductor devices and defects on the silicon-germanium interface, thereby improving the applicability of nanosheets and the quality of devices.
Smart Images

Figure CN116092941B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a nanosheet and a method for forming the same. Background Technology
[0002] With the development of semiconductor technology, the requirements for the integration density of semiconductor devices are becoming increasingly stringent. For two-dimensional or planar semiconductor devices, since their integration density is mainly determined by the projected area occupied by a unit memory cell on the silicon wafer surface, the integration density is greatly affected by the level of fine patterning technology. However, the extremely expensive process equipment used to improve pattern fineness sets a practical limit on increasing the integration density of two-dimensional or planar semiconductor devices. To overcome this limitation, three-dimensional structures, represented by fin gates and nanosheets (also known as nanostrips), are likely to replace traditional planar structures and become the mainstream structures below the 22-nanometer node.
[0003] In existing nanosheet manufacturing technologies, alternating silicon and sacrificial silicon-germanium layers are typically used to create a stacked structure. However, germanium in the sacrificial silicon-germanium layer diffuses into the silicon, causing compressive stress in the channels of the subsequently formed semiconductor devices due to the presence of germanium. Furthermore, defects easily form at the silicon-germanium interface, leading to the creation / recombination trap centers, which affect the yield and quality of the semiconductor devices. Summary of the Invention
[0004] The technical problem solved by this invention is to provide a nanosheet and a method for forming the same, which can effectively solve the problems of compressive stress in the channel of semiconductor devices and defects at the interface between silicon and silicon-germanium.
[0005] To address the aforementioned technical problems, embodiments of the present invention provide a method for forming nanosheets, comprising: providing a semiconductor substrate; forming an initial stacked layer on the surface of the semiconductor substrate, the initial stacked layer comprising alternating layers of sacrificial oxide and sacrificial nitride; forming a plurality of trenches penetrating the initial stacked layer and exposing the surface of the semiconductor substrate, the trenches dividing the initial stacked layer into a plurality of regions; forming an oxide layer within the trenches; forming one or more through-grooves in each region, the through-grooves penetrating the initial stacked layer and exposing the surface of the semiconductor substrate; removing sacrificial nitride layers in the initial stacked layer in contact with the through-grooves; forming an epitaxial growth structure within the through-grooves and in the space exposed after removing the sacrificial nitride layers to obtain a nanosheet stacked layer; wherein the trenches and the through-grooves are located at locations other than the nanostrip formation locations on the nanosheets.
[0006] Optionally, the forming method further includes: performing anisotropic etching on the nanosheet stack to form multiple nanostrips; wherein the etching depth of the anisotropic etching is greater than or equal to the thickness of the initial stack, and the locations of the trenches and the through-grooves are both etched in the etching process.
[0007] Optionally, the through groove in a single region is selected from: a single through groove; a single through groove and one or more through holes; or one or more through holes.
[0008] Optionally, the direction of the through groove is parallel to the direction of the groove.
[0009] Optionally, removing the sacrificial nitride layer in the initial stacked layer that contacts the through-groove includes: using an isotropic etching process to remove the sacrificial nitride layer in the initial stacked layer that contacts the through-groove.
[0010] Optionally, the semiconductor substrate is a silicon substrate; forming an epitaxial growth structure in the through-groove includes: forming a silicon epitaxial structure in the through-groove using an epitaxial growth process.
[0011] Optionally, the material of the oxide layer is the same as the material of the sacrificial oxide layer.
[0012] To address the aforementioned technical problems, embodiments of the present invention provide a nanosheet, comprising: a semiconductor substrate; an initial stacked layer located on the surface of the semiconductor substrate, the initial stacked layer comprising alternating layers of sacrificial oxide and sacrificial nitride; a plurality of trenches penetrating the initial stacked layer and exposing the surface of the semiconductor substrate, and the trenches dividing the initial stacked layer into a plurality of regions; an oxide layer located within the trenches; one or more through-grooves located within each region, the through-grooves penetrating the initial stacked layer and exposing the surface of the semiconductor substrate; and a nanosheet stacked layer formed by removing the sacrificial nitride layer from the initial stacked layer in contact with the through-grooves, and then forming an epitaxial growth structure in the space exposed after removing the sacrificial nitride layer and within the through-grooves; wherein the trenches and the through-grooves are located at locations other than the nanostrip formation locations on the nanosheet.
[0013] Optionally, the through groove in a single region is selected from: a single through groove; a single through groove and one or more through holes; or one or more through holes.
[0014] Optionally, the direction of the through groove is parallel to the direction of the groove.
[0015] Compared with the prior art, the technical solution of the embodiments of the present invention has the following beneficial effects:
[0016] In this embodiment of the invention, by using alternating stacked multilayer sacrificial oxide layers and multilayer sacrificial nitride layers instead of the sacrificial silicon-germanium layers in the prior art, the diffusion of germanium from the sacrificial silicon-germanium layers into the silicon layers can be effectively avoided, as can the formation of silicon-germanium interfaces. This effectively solves the problems of compressive stress in the channels of semiconductor devices and defects at the silicon-germanium interfaces. Furthermore, by forming multiple trenches and forming oxide layers within the trenches, the initial stacked layer can be divided into multiple regions and oxide layers can be formed as supports. By forming through-holes, the sacrificial nitride layers can be removed, and epitaxial growth structures can be formed in the exposed spaces. This results in a nanosheet stacked layer with alternating stacked epitaxial growth structures and sacrificial oxide layers, providing a foundation for the subsequent formation of nanosheet devices and improving the quality of semiconductor devices.
[0017] Furthermore, the nanosheet stack is subjected to anisotropic etching to form multiple nanostrips. The etching depth of the anisotropic etching process is greater than or equal to the thickness of the initial stack. The locations of the trenches and the through-grooves are etched during the etching process, thereby forming multiple nanostrips with alternating stacks of epitaxial growth structures and sacrificial oxide layers on the nanosheet. Since the trenches and the through-grooves are located at locations other than the nanostrip formation locations on the nanosheet, the support material between the previously divided regions and the epitaxial material in the through-grooves can be removed, making the nanosheets forming the nanostrips structurally consistent with conventional nanosheets, thus increasing the applicability of the nanosheets in this embodiment of the invention.
[0018] Furthermore, the through groove in a single area is selected from: a single through groove; a single through groove and one or more through holes; one or more through holes, so that an appropriate through groove can be formed according to specific needs.
[0019] Furthermore, the direction of the through groove is parallel to the direction of the trench, which can reduce the possibility of the through groove intersecting with the trench and effectively maintain the supporting strength of the supporting material between the previously divided areas.
[0020] Furthermore, the material of the oxide layer is the same as that of the sacrificial oxide layer, which helps to reduce the complexity of research and development and processes. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of a cross-sectional structure of a nanosheet in the prior art;
[0022] Figure 2 This is a schematic flowchart of a method for forming nanosheets according to an embodiment of the present invention;
[0023] Figures 3 to 9 This is a schematic diagram of the device cross-sectional structure corresponding to each step in a method for forming nanosheets according to an embodiment of the present invention. Attached image description:
[0025] Semiconductor substrate 10; sacrificial silicon-germanium layer 111; silicon layer 112; semiconductor substrate 20; sacrificial oxide layer 211; sacrificial nitride layer 212; trench 22; oxide layer 23; through trench 24; epitaxial growth structure 25; nanostrip 26; nanostrip sacrificial oxide layer 261; nanostrip epitaxial layer 262. Detailed Implementation
[0026] In existing nanosheet manufacturing technologies, silicon layers and sacrificial silicon-germanium layers are typically used for epitaxy to obtain a stacked structure.
[0027] Reference Figure 1 , Figure 1 This is a schematic diagram of a cross-sectional structure of a nanosheet in the prior art.
[0028] like Figure 1 As shown, a stacked layer is formed on the surface of the semiconductor substrate 10. The stacked layer includes alternating layers of sacrificial silicon-germanium layers 111 and silicon layers 112. The stacked layer is etched to obtain multiple nanostrips perpendicular to the semiconductor substrate 10.
[0029] Each nanostrip contains alternating adjacent sacrificial silicon-germanium (SiG) and silicon materials. This process is prone to germanium diffusion from the sacrificial SiG to the silicon, and defects can also occur at the interface between the sacrificial SiG and silicon materials. In subsequent processes, semiconductor devices are formed on the nanostrips, with the silicon layer forming the channels for these devices. Due to the diffusion of SiG, compressive stress exists in the channels, and defects at the silicon interface can create recombination trap centers, affecting the yield and quality of the semiconductor devices.
[0030] In this embodiment of the invention, by using alternating stacked multilayer sacrificial oxide layers and multilayer sacrificial nitride layers instead of the sacrificial silicon-germanium layers in the prior art, the diffusion of germanium from the sacrificial silicon-germanium layers into the silicon layers can be effectively avoided, as can the formation of silicon-germanium interfaces. This effectively solves the problems of compressive stress in the channel of semiconductor devices and defects at the silicon-germanium interface. Furthermore, by forming multiple trenches and forming oxide layers in the trenches, the initial stacked layer can be divided into multiple regions and oxide layers can be formed as supports. By forming through trenches, the sacrificial nitride layer can be removed and an epitaxial growth structure can be formed in the exposed space, thereby obtaining a nanosheet stacked layer with alternating stacked epitaxial growth structures and sacrificial oxide layers, providing a foundation for the subsequent formation of nanosheet devices.
[0031] To make the above-mentioned objectives, features and beneficial effects of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0032] Reference Figure 2 , Figure 2This is a schematic flowchart illustrating a method for forming nanosheets according to an embodiment of the present invention. The method for forming nanosheets may include steps S21 to S26:
[0033] Step S21: Provide a semiconductor substrate and form an initial stacked layer on the surface of the semiconductor substrate, the initial stacked layer comprising alternating stacked multilayer sacrificial oxide layers and multilayer sacrificial nitride layers;
[0034] Step S22: Form a plurality of trenches that penetrate the initial stacked layer and expose the surface of the semiconductor substrate, and the trenches divide the initial stacked layer into a plurality of regions;
[0035] Step S23: Form an oxide layer in the trench;
[0036] Step S24: Form one or more through-holes in each region, the through-holes penetrating the initial stacked layer and exposing the surface of the semiconductor substrate;
[0037] Step S25: Remove the sacrificial nitride layer from the initial stacked layer that contacts the through-groove;
[0038] Step S26: An epitaxial growth structure is formed in the through-groove and in the space exposed after the sacrificial nitride layer is removed, to obtain a stacked nanosheet layer.
[0039] The trenches and the through-grooves are located at positions other than the nanostrip formation locations on the nanosheet.
[0040] The following combination Figures 3 to 9 The steps described above will be explained.
[0041] Figures 3 to 9 This is a schematic diagram of the device cross-sectional structure corresponding to each step in a method for forming nanosheets according to an embodiment of the present invention.
[0042] Reference Figure 3 A semiconductor substrate 20 is provided, and an initial stacked layer is formed on the surface of the semiconductor substrate 20, the initial stacked layer comprising alternating stacked multilayer sacrificial oxide layers 211 and multilayer sacrificial nitride layers 212.
[0043] The semiconductor substrate 20 can be a silicon substrate or a germanium substrate. The semiconductor substrate 20 can also be a silicon substrate on an insulator or a germanium substrate on an insulator, or a substrate with an epitaxial layer (Epilayer) grown on it.
[0044] In this embodiment of the invention, a silicon substrate or a silicon substrate on an insulator can be used to take advantage of the good epitaxial growth capability of silicon material to form a higher quality epitaxial growth structure in subsequent process steps.
[0045] It should be noted that subsequent process steps include forming an epitaxial growth structure, therefore the material of the semiconductor substrate 20 can be a suitable material capable of epitaxial growth.
[0046] The material of the sacrificial oxide layer 211 can be silicon oxide, such as SiO2.
[0047] Without limitation, the material of the sacrificial oxide layer 211 can also be other suitable materials, such as germanium oxide.
[0048] The material of the sacrificial nitride layer 212 can be silicon nitride, such as Si3N4.
[0049] Without limitation, the material of the sacrificial nitride layer 212 can also be other suitable materials, such as germanium nitride.
[0050] In this embodiment of the invention, by using alternating stacked multilayer sacrificial oxide layers and multilayer sacrificial nitride layers instead of the sacrificial silicon-germanium layers in the prior art, the diffusion of germanium from the sacrificial silicon-germanium layers into the silicon layers can be effectively avoided, and the formation of silicon-germanium interfaces can also be avoided, effectively solving the problems of compressive stress in the channel of semiconductor devices and defects at the silicon-germanium interface.
[0051] Reference Figure 4 Multiple trenches 22 are formed, which penetrate the initial stacked layer and expose the surface of the semiconductor substrate 20, and divide the initial stacked layer into multiple regions, such as... Figure 4 The regions shown are A1, A2, etc.
[0052] The shape of each region can be polygonal, such as rectangle, triangle, hexagon, octagon, etc.
[0053] The groove 22 can be located at a position other than the nanostrip formation position on the nanosheet, so that the influence of the support material in the groove 22 can be avoided when the nanostrip is formed subsequently.
[0054] Reference Figure 5 In the trench 22 (refer to) Figure 4 An oxide layer 23 is formed inside.
[0055] Specifically, the oxide layer 23 can be formed using chemical vapor deposition or other suitable processes.
[0056] Non-limitingly, the process for forming oxide layer 23 can be selected from: plasma enhanced chemical vapor deposition (PECVD), subatmosphere chemical vapor deposition (SACVD), in-situ steam generation (ISSG) (also known as internal steam oxidation), atomic layer deposition (ALD), and flowable chemical vapor deposition (FCVD).
[0057] Furthermore, the material of the oxide layer 23 can be the same as the material of the sacrificial oxide layer 211.
[0058] The oxide layer 23 can be made of silicon oxide, such as SiO2.
[0059] Without limitation, the oxide layer 23 can also be made of other suitable materials, such as germanium oxide.
[0060] In this embodiment of the invention, the material of the oxide layer 23 is the same as that of the sacrificial oxide layer 211, which helps to reduce the complexity of research and development and processes.
[0061] In this embodiment of the invention, by forming a plurality of trenches 22 and forming an oxide layer 23 within the trenches 22, the initial stacked layer can be divided into a plurality of regions and an oxide layer 23 can be formed as a support.
[0062] Reference Figure 6 One or more through-grooves 24 are formed in each region, the through-grooves 24 penetrating the initial stacked layer and exposing the surface of the semiconductor substrate 20.
[0063] The through-groove 24 can be located at a position other than the nano-strip formation position on the nanosheet, so that the influence of the epitaxial growth material in the through-groove 24 can be avoided when forming nano-strips later.
[0064] Furthermore, the through groove 24 in a single region can be selected from: a single through groove; a single through groove and one or more through holes; or one or more through holes.
[0065] In this embodiment of the invention, the through groove 24 in a single region is selected from: a single through groove; a single through groove and one or more through holes; one or more through holes, so that an appropriate through groove 24 can be formed according to specific needs.
[0066] In one specific embodiment of the present invention, the through groove 24 in a single area may be a single through trench.
[0067] Specifically, compared to using multiple through trenches in a single area, which may pose a risk that the support material between different areas cannot support the entire area, using a single through trench in a single area can maintain the support strength of the support material for the current area and provide epitaxial growth space for the epitaxial growth structure in subsequent processes.
[0068] In another specific embodiment of the present invention, the size of the through hole in a single region may be greater than a preset size (for example, the diameter of the through hole may be greater than a preset diameter), and / or, the arrangement density of the through holes in a single region may be greater than a preset density.
[0069] Specifically, compared to using smaller, lower-density through-holes in a single region, using larger and / or higher-density through-holes in a single region can provide more epitaxial growth space in the epitaxial growth structure in subsequent processes, which helps to improve epitaxial growth efficiency.
[0070] Furthermore, the direction of the through groove can be parallel to the direction of the groove 22.
[0071] In this embodiment of the invention, the direction of the through groove is parallel to the direction of the groove 22, thereby reducing the possibility of the through groove intersecting with the groove 22 and effectively maintaining the supporting strength of the supporting material between the previously divided areas.
[0072] Reference Figure 7 Remove the sacrificial nitride layer 212 from the initial stacked layer that contacts the through groove 24 (see reference). Figure 6 ).
[0073] Furthermore, the step of removing the sacrificial nitride layer 212 in the initial stacked layer that contacts the through-groove 24 may include: using an isotropic etching process to remove the sacrificial nitride layer 212 in the initial stacked layer that contacts the through-groove 24.
[0074] Furthermore, the isotropic etching process can employ a wet etching process, thereby removing the sacrificial nitride layer 212 within the area of the opening with a limited area as much as possible.
[0075] Reference Figure 8In the through groove 24 (refer to) Figure 7 ) and removal of the sacrificial nitride layer 212 (refer to Figure 6 The exposed space then forms an epitaxial growth structure 25 to obtain a stacked layer of nanosheets.
[0076] In this embodiment of the invention, by forming a through groove 24, the sacrificial nitride layer 212 can be removed and an epitaxial growth structure 25 can be formed in the exposed space, thereby obtaining a stacked layer of nanosheets with alternating stacking of epitaxial growth structure 25 and sacrificial oxide layer 212, providing a basis for the subsequent formation of nanostrips.
[0077] Furthermore, the semiconductor substrate 20 may be a silicon substrate; forming an epitaxial growth structure 25 within the through-groove 24 includes: forming a silicon epitaxial structure 25 within the through-groove 24 using an epitaxial growth process.
[0078] It should be noted that, in another specific embodiment, the semiconductor substrate 20 may also be a germanium substrate; forming an epitaxial growth structure 25 in the through-groove 24 includes: forming a germanium epitaxial structure in the through-groove 24 using an epitaxial growth process.
[0079] In this embodiment of the invention, by using alternating stacked multilayer sacrificial oxide layers 211 and multilayer sacrificial nitride layers 212 instead of the sacrificial silicon-germanium layers in the prior art, the diffusion of germanium from the sacrificial silicon-germanium layers into the silicon layers can be effectively avoided, as can the formation of silicon-germanium interfaces. This effectively solves the problems of compressive stress in the channel of semiconductor devices and defects at the silicon-germanium interface. Furthermore, by forming multiple trenches 22 and forming oxide layers 23 in the trenches, the initial stacked layer can be divided into multiple regions and oxide layers 23 can be formed as supports. By forming through trenches 24, the sacrificial nitride layers 212 can be removed and epitaxial growth structures 25 can be formed in the exposed space, thereby obtaining a nanosheet stacked layer in which epitaxial growth structures 25 and sacrificial oxide layers 212 are alternately stacked, providing a foundation for the subsequent formation of nanosheet devices.
[0080] Reference Figure 9 The nanosheet stack is anisotropically etched to form multiple nanostrips 26. Each nanostrip 26 may include alternating stacked nanostrip sacrificial oxide layers 261 and nanostrip epitaxial layers 262.
[0081] The etching depth of the anisotropic etching process can be greater than or equal to the thickness of the initial stacked layer, and the locations of the trench 22 and the through-groove 24 are both etched in the etching process.
[0082] Furthermore, the anisotropic etching process can be performed using a dry etching process, with etching directed toward the semiconductor substrate 20.
[0083] In this embodiment of the invention, the nanosheet stack is subjected to anisotropic etching to form multiple nanostrips 26. The etching depth of the anisotropic etching is greater than or equal to the thickness of the initial stack. The locations of the trenches 22 and the through-grooves 24 are etched during the etching process, thereby forming multiple alternating stacked nanostrip sacrificial oxide layers 261 and nanostrip epitaxial layers 262 on the nanosheet. Since the trenches 22 and the through-grooves 24 are located at locations other than the nanostrip formation locations on the nanosheet, the support material between the previously divided regions and the epitaxial material in the through-grooves 24 can be removed, making the nanosheets forming the nanostrips 26 structurally consistent with conventional nanosheets, thus increasing the applicability of the nanosheets in this embodiment of the invention.
[0084] In this embodiment of the invention, a nanosheet is also disclosed, with reference to Figure 8 The structure may include: a semiconductor substrate 20; an initial stacked layer located on the surface of the semiconductor substrate 20, the initial stacked layer comprising alternating layers of sacrificial oxide layers 211 and layers of sacrificial nitride layers 212; a plurality of trenches 22 penetrating the initial stacked layer and exposing the surface of the semiconductor substrate 20, and the trenches 22 dividing the initial stacked layer into a plurality of regions; an oxide layer 23 located within the trenches 22; one or more through-grooves 24 located within each region, the through-grooves 24 penetrating the initial stacked layer and exposing the surface of the semiconductor substrate 20; and a nanosheet stacked layer formed by removing the sacrificial nitride layers 212 from the initial stacked layer in contact with the through-grooves 24, and forming an epitaxial growth structure 25 in the space exposed after removing the sacrificial nitride layers 212 and within the through-grooves 24; wherein the trenches 22 and the through-grooves 24 are located at locations other than the nanostrip formation locations on the nanosheets.
[0085] Furthermore, the through groove 24 in a single region is selected from: a single through groove; a single through groove and one or more through holes; or one or more through holes.
[0086] Furthermore, the direction of the through groove is parallel to the direction of the groove 22.
[0087] In this embodiment of the invention, by using alternating stacked multilayer sacrificial oxide layers 211 and multilayer sacrificial nitride layers 212 instead of the sacrificial silicon-germanium layers in the prior art, the diffusion of germanium from the sacrificial silicon-germanium layers into the silicon layers can be effectively avoided, as can the formation of silicon-germanium interfaces. This effectively solves the problems of compressive stress in the channel of semiconductor devices and defects at the silicon-germanium interface. Furthermore, by forming multiple trenches 22 and forming oxide layers 23 in the trenches, the initial stacked layer can be divided into multiple regions and oxide layers 23 can be formed as supports. By forming through trenches 24, the sacrificial nitride layers 212 can be removed and epitaxial growth structures 25 can be formed in the exposed space, thereby obtaining a nanosheet stacked layer in which epitaxial growth structures 25 and sacrificial oxide layers 212 are alternately stacked, providing a foundation for the subsequent formation of nanosheet devices.
[0088] For the principles, specific implementation, and beneficial effects of this nanosheet, please refer to the previous description of the nanosheet formation method; it will not be repeated here.
[0089] It should be understood that the term "and / or" in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the character " / " in this article indicates that the preceding and following related objects have an "or" relationship.
[0090] In the embodiments of this application, "multiple" refers to two or more.
[0091] The descriptions of "first," "second," etc., appearing in the embodiments of this application are for illustrative purposes and to distinguish the objects being described. They have no order and do not indicate any special limitation on the number of devices in the embodiments of this application, nor do they constitute any limitation on the embodiments of this application.
[0092] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A method for forming nanosheets, characterized in that, include: A semiconductor substrate is provided, and an initial stacked layer is formed on the surface of the semiconductor substrate, the initial stacked layer comprising alternating stacked multilayer sacrificial oxide layers and multilayer sacrificial nitride layers; Multiple trenches are formed, the trenches penetrating the initial stacked layer and exposing the surface of the semiconductor substrate, and the trenches divide the initial stacked layer into multiple regions; An oxide layer is formed within the trench; One or more through-grooves are formed in each region, the through-grooves penetrating the initial stacked layer and exposing the surface of the semiconductor substrate; Remove the sacrificial nitride layer from the initial stacked layer that contacts the through-groove; An epitaxial growth structure is formed within the through-groove and in the space exposed after the sacrificial nitride layer is removed, to obtain a stacked layer of nanosheets; The grooves and the through grooves are located at positions other than the nanostrip formation locations on the nanosheet; Also includes: The nanosheet stack is subjected to anisotropic etching to form multiple nanostrips, each nanostrip including alternating stacked nanostrip sacrificial oxide layers and nanostrip epitaxial layers; The etching depth of the anisotropic etching process is greater than or equal to the thickness of the initial stacked layer, and the locations of the trenches and the through-grooves are both etched during the etching process.
2. The forming method according to claim 1, characterized in that, The through-slots within a single area are selected from: Single through trench; A single through-groove and one or more through holes; One or more through holes.
3. The forming method according to claim 2, characterized in that, The direction of the through trench is parallel to the direction of the trench.
4. The forming method according to claim 1, characterized in that, Removing the sacrificial nitride layer from the initial stack layer in contact with the through-groove includes: An isotropic etching process is used to remove the sacrificial nitride layer in the initial stacked layer that is in contact with the through-groove.
5. The forming method according to claim 1, characterized in that, The semiconductor substrate is a silicon substrate; An epitaxial growth structure is formed within the through-groove, including: A silicon epitaxial structure is formed within the through-groove using an epitaxial growth process.
6. The forming method according to claim 1, characterized in that, The material of the oxide layer is the same as that of the sacrificial oxide layer.
7. A nanosheet, characterized in that, include: Semiconductor substrate; An initial stacked layer is located on the surface of the semiconductor substrate, the initial stacked layer comprising alternating stacked multiple layers of sacrificial oxide and multiple layers of sacrificial nitride; Multiple trenches penetrate the initial stacked layer and expose the surface of the semiconductor substrate, and the trenches divide the initial stacked layer into multiple regions; An oxide layer is located within the trench; One or more through-holes are located in each region, the through-holes penetrating the initial stacked layer and exposing the surface of the semiconductor substrate; The nanosheet stack is obtained by removing the sacrificial nitride layer in the initial stack that is in contact with the through groove, and then forming an epitaxial growth structure in the space exposed after removing the sacrificial nitride layer and in the through groove. The grooves and the through grooves are located at positions other than the nanostrip formation locations on the nanosheet; Also includes: Multiple nanostrips are obtained by anisotropic etching of the stacked nanosheet layers. Each nanostrip includes alternating stacked nanostrip sacrificial oxide layers and nanostrip epitaxial layers. The etching depth of the anisotropic etching process is greater than or equal to the thickness of the initial stacked layer, and the locations of the trenches and the through-grooves are both etched during the etching process.
8. The nanosheet according to claim 7, characterized in that, The through-slots within a single area are selected from: Single through trench; A single through-groove and one or more through holes; One or more through holes.
9. The nanosheet according to claim 8, characterized in that, The direction of the through trench is parallel to the direction of the trench.
Citation Information
Patent Citations
3D NAND memory device and manufacturing method thereof
CN111244096A